Production process of high-stability zirconium oxide fibrofelt
By using specific ingredients in the soaking slurry and high-temperature sintering technology in the production process of zirconia fiber felt, the problem of insufficient toughness of zirconia powder fiber felt is solved and its deformation resistance and stability in high-temperature environments are improved.
Patent Information
- Application Number
- CN202410824508.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-25
AI Technical Summary
The existing zirconia powder fiber mat has insufficient toughness and poor deformation resistance, making it difficult to maintain stability in high temperature environments.
Zirconium sol, yttrium sol, white latex, toughening agent, chromium chloride, calcium stearate and other ingredients in the soaking slurry are used to improve the strength and stability of the zirconia fiber felt through soaking and high-temperature sintering processes.
The deformation resistance and stability of the zirconia fiber mat are significantly improved, making it more reliable for use in high temperature environments.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zirconia fiber felt, in particular to a production process of high-stability zirconia fiber felt. Background Art
[0002] Compared with other types of inorganic fiber materials such as zirconia aluminum fiber, mullite fiber and aluminum silicate fiber, zirconia fiber has high melting point, large thermal resistance coefficient, good burning resistance, can maintain good fiber shape at 2500℃ in the atmosphere, acid and alkali chemical corrosion resistance, low vapor pressure at high temperature, etc. Therefore, zirconia fiber can be used as a key basic material for ultra-high temperature thermal insulation filling, composite, structural reinforcement or toughening. In addition, it can be used to manufacture and process various zirconia fiber products, mainly including zirconia fiber felt, fiber blanket, zirconia fiber paper, zirconia fiber cloth and rigid zirconia fiber products, etc. According to its shape and structure Due to its different structures, it is used in environments with different requirements. Since the thermal expansion coefficient of zirconia fiber is similar to that of many metals, alloys, glass, concrete and other materials, it can be used as a reinforcing agent for various matrices such as metals, ceramics, glass, resins, cement, etc. It has unique advantages in impact-resistant high-temperature thermal insulation composite materials, etc. It can also be used for lasers, fuel cell diaphragms, satellites and aircraft engine components, and filtration of high-temperature or chemically corrosive gases or catalyst carriers. Because of its ultra-high temperature resistance, low thermal conductivity, high-temperature oxidation resistance, and strong corrosion resistance, it is widely used in cutting-edge military science and technology fields and civilian industrial fields.
[0003] After searching, a patent with announcement number CN104671812B discloses a method for producing a stable zirconium oxide powder fiber felt. The method uses fiber felt as a carrier, which is first soaked in a saturated zirconium oxide solution, then treated with zirconium sol on the surface, and then sintered at a high temperature to obtain zirconium oxide powder fiber felt. The production method has the characteristics of simple production process, low production cost, no need for complex equipment, and environmental friendliness. The prepared zirconium oxide powder fiber felt has high strength and high temperature resistance, and can be directly used in ultra-high temperature environments. Moreover, fiber felt is used as a base material. Although the process is simple, its toughness is insufficient and its deformation resistance is poor during use. Therefore, the present invention proposes a production process for high-stability zirconium oxide fiber felt. Summary of the invention
[0004] The purpose of the present invention is to provide a production process of high-stability zirconia fiber felt to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a production process of high-stability zirconia fiber felt, comprising the following steps:
[0006] S1. Weigh the raw materials according to the formula, and place the raw materials in a mixing device to disperse and prepare the soaking slurry. After the preparation is completed, transfer the soaking slurry to a slurry tank for standby use;
[0007] S2, selecting a zirconium oxide fiber base material, placing all of the zirconium oxide fiber base material in a slurry tank to fully absorb the soaking slurry, and pumping air into the slurry tank during this process to accelerate the absorption efficiency, thereby obtaining a zirconium oxide fiber soaking liquid;
[0008] S3, filtering the zirconium oxide fiber soaking liquid in S2 to remove excess water, and evenly spreading the remaining slurry on the material plate to shape it, and after the slurry is dried and formed, sintering it at high temperature to form a zirconium oxide fiber felt;
[0009] The raw materials for soaking the slurry in step S1 include: 3-5 parts of zirconium sol, 1-2 parts of yttrium sol, 1-5 parts of filler, 1-10 parts of foaming agent, 3-9 parts of polyvinyl alcohol, 2-3 parts of white latex, 1-5 parts of toughening agent, 11-19 parts of chromium chloride, 5-7 parts of calcium stearate and 75-85 parts of water.
[0010] Preferably, the preparation method of the soaking slurry in step S1 is:
[0011] A1. Weigh the corresponding amounts of water, zirconium sol, yttrium sol and white latex according to the formula, and mix them in a material tank until the zirconium sol, yttrium sol and white latex are completely dispersed in the water for later use;
[0012] A2, weigh filler, foaming agent, polyvinyl alcohol, toughening agent, chromium chloride and calcium stearate, and place the above raw materials in a material tank and the solution in A1, and mix them again. After the mixture starts to foam, the preparation of the soaking slurry is completed.
[0013] Preferably, the length of the zirconia fiber base material in step S1 is 1-10 mm, preferably 1-3 mm.
[0014] Preferably, in step S2, the zirconia fiber base material absorbs the soaking slurry for 12-36 hours.
[0015] Preferably, the gas pumped into the slurry pool in step S2 is an inert gas, preferably argon, and the pumping time is 2-4 hours.
[0016] Preferably, the slurry is spread to a thickness of 2-4 mm in step S3, and the difference in spreading thickness is less than 0.3 mm.
[0017] Preferably, the sintering temperature in step S3 is 900-1600° C., and the heating rate during the sintering process is 3-5° C. / s, and the sintering time is 3-6 hours.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: by placing the zirconium oxide fiber in an immersion slurry for adsorption and preparing the zirconium oxide fiber felt through a process of shaping and sintering, its texture strength can be improved, thereby ensuring its anti-deformation force during use, and zirconium sol, yttrium sol and white latex are added to the immersion slurry to ensure that the stable zirconium oxide fiber will not be lost during the sintering process, and the added toughening agent, chromium chloride and calcium stearate can improve the strength of the prepared zirconia fiber felt to ensure the stability of the zirconia fiber felt during use. DETAILED DESCRIPTION
[0019] The present invention provides a technical solution: a production process of high-stability zirconia fiber felt, comprising the following steps:
[0020] S1. Weigh the raw materials according to the formula, and place the raw materials in a mixing device to disperse and prepare the soaking slurry. After the preparation is completed, transfer the soaking slurry to a slurry tank for standby use;
[0021] S2, selecting a zirconium oxide fiber base material, placing all of the zirconium oxide fiber base material in a slurry tank to fully absorb the soaking slurry, and pumping air into the slurry tank during this process to accelerate the absorption efficiency, thereby obtaining a zirconium oxide fiber soaking liquid;
[0022] S3, filtering the zirconium oxide fiber soaking liquid in S2 to remove excess water, and evenly spreading the remaining slurry on the material plate to shape it, and after the slurry is dried and formed, sintering it at high temperature to form a zirconium oxide fiber felt;
[0023] The zirconium oxide fiber felt is prepared by placing the zirconium oxide fiber in an immersion slurry for adsorption and shaping and sintering, so that its texture strength can be improved, thereby ensuring its deformation resistance during use.
[0024] The raw materials for soaking the slurry in step S1 include: 3-5 parts of zirconium sol, 1-2 parts of yttrium sol, 1-5 parts of filler, 1-10 parts of foaming agent, 3-9 parts of polyvinyl alcohol, 2-3 parts of white latex, 1-5 parts of toughening agent, 11-19 parts of chromium chloride, 5-7 parts of calcium stearate and 75-85 parts of water.
[0025] Preferably, the preparation method of the soaking slurry in step S1 is:
[0026] A1. Weigh the corresponding amounts of water, zirconium sol, yttrium sol and white latex according to the formula, and mix them in a material tank until the zirconium sol, yttrium sol and white latex are completely dispersed in the water for later use;
[0027] A2, weighing filler, foaming agent, polyvinyl alcohol, toughening agent, chromium chloride and calcium stearate, and placing the above raw materials in a material tank and the solution in A1, and mixing again, and completing the preparation of the soaking slurry after the mixture is foamed;
[0028] Zirconium sol, yttrium sol and white latex are added to the soaking slurry to ensure that the stable zirconia fiber will not be lost during the sintering process. The added toughening agent, chromium chloride and calcium stearate can improve the strength of the prepared zirconia fiber felt to ensure the stability of the zirconia fiber felt.
[0029] Preferably, the length of the zirconia fiber base material in step S1 is 1-10 mm, preferably 1-3 mm; the time for the zirconia fiber base material to absorb the soaking slurry in step S2 is 12-36 hours; the gas pumped into the slurry pool in step S2 is an inert gas, preferably argon, and the pumping time is 2-4 hours; the slurry spreading thickness in step S3 is 2-4 mm, and the spreading thickness difference is less than 0.3 mm; the sintering temperature in step S3 is 900-1600°C, and the heating rate during the sintering process is 3-5°C / s, and the sintering time is 3-6 hours.
[0030] Embodiment 1:
[0031] According to the formula, 75 parts of water, 3 parts of zirconium sol, 1 part of yttrium sol and 2 parts of white latex were weighed and mixed in a material tank. After the zirconium sol, yttrium sol and white latex were completely dispersed in the water, 1 part of filler, 1 part of foaming agent, 3 parts of polyvinyl alcohol, 1 part of toughening agent, 11 parts of chromium chloride and 5 parts of calcium stearate were weighed and placed in a material tank with the solution in A1 and mixed again. After the mixture was foamed, the preparation of the soaking slurry was completed. The soaking slurry was then transferred to the slurry tank for use. Zirconia fibers with a length of 1-10 mm were selected. Place all the zirconium oxide fiber base materials in a slurry pool to fully absorb the soaking slurry for 18 hours, and pump argon into the slurry pool for 2 hours in the process to accelerate the absorption efficiency, and obtain the zirconium oxide fiber soaking liquid. Filter the zirconium oxide fiber soaking liquid to remove excess water, and spread the remaining slurry evenly on the material board for shaping, and control the spreading thickness to be 2mm. After the slurry is dried and formed, it is sintered at a high temperature for 3 hours, and the maximum sintering temperature is controlled to be 1200℃. The heating rate during the sintering process is 3℃ / s, thereby forming the required zirconia fiber felt.
[0032] Embodiment 2:
[0033] According to the formula, 85 parts of water, 5 parts of zirconium sol, 2 parts of yttrium sol and 3 parts of white latex were weighed and mixed in a material tank. After the zirconium sol, yttrium sol and white latex were completely dispersed in the water, they were set aside. 3 parts of filler, 5 parts of foaming agent, 6 parts of polyvinyl alcohol, 3 parts of toughening agent, 15 parts of chromium chloride and 6 parts of calcium stearate were weighed and placed in a material tank with the solution in A1 and mixed again. After the mixture was foamed, the preparation of the soaking slurry was completed. The soaking slurry was then transferred to a slurry tank for use. Zirconia fibers with a length of 1-10 mm were selected. The zirconia fiber base material is placed in a slurry pool to fully absorb the soaking slurry for 35 hours, and argon is pumped into the slurry pool for 4 hours in the process to accelerate the absorption efficiency, so as to obtain the zirconia fiber soaking liquid. The zirconia fiber soaking liquid is filtered to remove excess water, and the remaining slurry is evenly spread on the material board for shaping, and the spreading thickness is controlled to be 4mm. After the slurry is dried and formed, it is sintered at a high temperature for 4 hours, and the maximum sintering temperature is controlled to be 1400℃. The heating rate during the sintering process is 4℃ / s, so as to form the required zirconia fiber felt.
[0034] Although the embodiments of the present invention have been shown and described herein, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process of high stability zirconia fiber felt, It is characterized in that The following steps are involved: S1. Weigh the raw materials according to the formula, and place the raw materials in a mixing device to disperse and prepare the soaking slurry. After the preparation is completed, transfer the soaking slurry to a slurry tank for standby use; S2, selecting a zirconium oxide fiber base material, placing all of the zirconium oxide fiber base material in a slurry tank to fully absorb the soaking slurry, and pumping air into the slurry tank during this process to accelerate the absorption efficiency, thereby obtaining a zirconium oxide fiber soaking liquid; S3, filtering the zirconium oxide fiber soaking liquid in S2 to remove excess water, and evenly spreading the remaining slurry on the material plate to shape it, and after the slurry is dried and formed, sintering it at high temperature to form a zirconium oxide fiber felt; The raw materials for soaking the slurry in step S1 include: 3-5 parts of zirconium sol, 1-2 parts of yttrium sol, 1-5 parts of filler, 1-10 parts of foaming agent, 3-9 parts of polyvinyl alcohol, 2-3 parts of white latex, 1-5 parts of toughening agent, 11-19 parts of chromium chloride, 5-7 parts of calcium stearate and 75-85 parts of water.
2. A production process for a high-stability zirconia fiber felt according to claim 1, Features: The preparation method of the soaking slurry in step S1 is: A1. Weigh the corresponding amounts of water, zirconium sol, yttrium sol and white latex according to the formula, and mix them in a material tank until the zirconium sol, yttrium sol and white latex are completely dispersed in the water for later use; A2, weigh filler, foaming agent, polyvinyl alcohol, toughening agent, chromium chloride and calcium stearate, and place the above raw materials in a material tank and the solution in A1, and mix them again. After the mixture starts to foam, the preparation of the soaking slurry is completed.
3. The production process of a high-stability zirconia fiber felt according to claim 1, Features: The length of the zirconia fiber base material in step S1 is 1-10 mm, preferably 1-3 mm.
4. The production process of a high-stability zirconia fiber felt according to claim 1, Features: In step S2, the zirconia fiber base material absorbs the soaking slurry for 12-36 hours.
5. The production process of a high-stability zirconia fiber felt according to claim 1, Features: The gas pumped into the slurry pool in step S2 is an inert gas, preferably argon, and the pumping time is 2-4 hours.
6. The production process of a high-stability zirconia fiber felt according to claim 1, Features: The slurry is spread to a thickness of 2-4 mm in step S3, and the difference in the spread thickness is less than 0.3 mm.
7. The production process of a high-stability zirconia fiber felt according to claim 1, Features: The sintering temperature in step S3 is 900-1600° C., and the heating rate during the sintering process is 3-5° C. / s, and the sintering time is 3-6 hours.
Citation Information
Patent Citations
Porous abrasive articles with agglomerated abrasives and method for making the agglomerated abrasives
CA2580657A1
Method for preparing hollow zirconium oxide fibers
CN106350898A
Phillipsite-containing thermal-insulation brick and preparation method thereof
CN107200561A
High-strength zirconia fiber felt prepared by impregnation method
CN111850816A
Calcium hexaluminate series refractory material, nanometer heat insulation plate, composite refractory material lining body structure body, preparation method and application of composite refractory material lining body structure body
CN115321974A