Three-dimensional porous Ti3C2Tx membrane material as well as preparation method and application thereof
By using surfactant F127 and Ti3C2Tx nanosheets to self-assemble and perform pyrolysis treatment, a three-dimensional interconnected pore structure is constructed, which solves the problem of uneven pore distribution within the three-dimensional porous Ti3C2Tx membrane material and improves its electrochemical performance and applicability. Suitable as electrode material for supercapacitors.
Patent Information
- Application Number
- CN202411140428.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the internal pores of the three-dimensional porous Ti3C2Tx membrane material are unevenly distributed, resulting in stacking and aggregation between Ti3C2Tx nanosheets, which limits its application in supercapacitor electrode materials.
The surfactant F127 is used as a soft template to self-assemble with Ti3C2Tx nanosheets. A film is formed through vacuum filtration and drying, and then pyrolysis is performed to decompose the surfactant to build a three-dimensional interconnected pore structure, which solves the problem of stacking and aggregation of nanosheets. question.
It achieves uniform pore distribution within the three-dimensional porous Ti3C2Tx membrane material, reduces stacking and aggregation between nanosheets, improves electrolyte penetration rate and electron/ion transport efficiency, has excellent electrochemical performance and toughness, and is suitable as a self-supporting Electrode materials.
Smart Images

Figure CN118782402A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of porous materials, and in particular relates to a three-dimensional porous Ti3C2T x Membrane material, preparation method and use thereof. Background Art
[0002] Ti3C2T x As a typical MXenes (new two-dimensional layered transition metal carbides, nitrides or carbonitrides) material, it has broad application prospects in the field of supercapacitor electrode materials due to its metal-like conductivity, redox reaction pseudocapacitance mechanism (high capacitance), high density (high volume capacitance), and adjustable surface terminal functional groups. x There are strong van der Waals forces between nanosheets, which are prone to self-stacking or aggregation during the electrode preparation process, resulting in a reduction in the active area of the nanosheets, hindered ion dynamic diffusion, and reduced electrolyte ion accessibility, thus inhibiting the Ti3C2T x Nanosheets self-stack or aggregate to optimize their performance. x The application and development of supercapacitors is crucial.
[0003] The construction of three-dimensional structure is to inhibit the Ti3C2T x A very effective way to self-stack or aggregate nanosheets. x Not only has two-dimensional Ti3C2T x The advantages of Ti3C2T are not only: (1) the large ion-accessible surface area and many active sites allow sufficient electrochemical reactions to occur; (2) the well-developed and interconnected porous structure provides abundant paths for the diffusion of electrolytes, and Ti3C2T x High conductivity enables rapid charge movement within the porous framework; (3) Abundant surface functional groups (-O, -OH, -F) can serve as binding sites for various organic and inorganic substances to create three-dimensional Ti3C2T3 structures of varying complexity and utility. x structure; (4) the three-dimensional conductive topology can ensure excellent charge transfer performance throughout the entire dense electrode volume.
[0004] However, the three-dimensional porous Ti3C2T prepared by the prior art x The pores inside the membrane are unevenly distributed, Ti3C2T x There is still stacking and aggregation between nanosheets, which limits their wide application as electrode materials in the energy field. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a three-dimensional porous Ti3C2T xA method for preparing a membrane material. The method comprises: x The nanosheets were added dropwise into the surfactant F127 solution and stirred, so that the surfactant F127 acted as a soft template and bonded with Ti3C2T x The nanosheets are self-assembled, and a membrane is formed after vacuum filtration and drying. The surfactant F127 in the membrane structure is decomposed into gas and discharged through pyrolysis to obtain a Ti3C2T3O3 interconnected pore structure. x Membrane material, solves the problem of three-dimensional porous Ti3C2T prepared by existing technology x The pores inside the membrane are unevenly distributed, Ti3C2T x There are problems of stacking and aggregation between nanosheets.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is: a three-dimensional porous Ti3C2T x The method for preparing a membrane material comprises the following steps:
[0007] Step 1: Ti3C2T x The nanosheet dispersion solution was added dropwise into the surfactant F127 solution and stirred to obtain a mixed solution;
[0008] Step 2: vacuum filter the mixed solution obtained in step 1 and form a membrane after drying;
[0009] Step 3: The film formed in step 2 is placed in a tube furnace for pyrolysis, and then cooled naturally to obtain a three-dimensional porous Ti3C2T x membrane material.
[0010] The present invention adopts surfactant F127 solution as a soft template for reacting with Ti3C2T x The nanosheets self-assembled, and the surfactant F127 was evenly distributed inside the membrane through stirring, vacuum filtration and drying. The surfactant F127 in the membrane was completely decomposed and removed by pyrolysis of the membrane, leaving the corresponding pores to obtain a three-dimensional porous Ti3C2T x Membrane material, where T x Surface functional groups.
[0011] The above-mentioned three-dimensional porous Ti3C2T x The method for preparing a membrane material is characterized in that the Ti3C2T x The concentration of the nanosheet dispersion solution is 0.5 mg / mL to 5 mg / mL.
[0012] The present invention controls Ti3C2T x The concentration range of the nanosheet dispersion solution is conducive to the realization of Ti3C2T xThe self-assembly process of nanosheets and surfactant F127 occurred, thus constructing a three-dimensional porous structure; Ti3C2T x When the concentration of the nanosheet dispersion solution is lower than 0.5 mg / mL, the membrane material is prone to breakage. x When the concentration of the nanosheet dispersion solution is higher than 5 mg / mL, the self-assembly process is not easy to occur, or there are fewer voids inside the membrane, which affects the performance of the material.
[0013] The above-mentioned three-dimensional porous Ti3C2T x The method for preparing a membrane material is characterized in that the concentration of the surfactant F127 solution in step 1 is 0.5 mg / mL to 10 mg / mL.
[0014] The present invention sets the concentration range of the surfactant F127 solution to make the three-dimensional porous structure of the prepared sample obvious. When the concentration of the surfactant F127 solution is lower than 0.5 mg / mL, it is difficult to form a porous structure on Ti3C2T x A large number of pores are constructed inside the membrane material to achieve a three-dimensional porous structure. A concentration higher than 10 mg / mL will cause the gas generated during the pyrolysis process to take away part of the Ti3C2T x Nanosheets make Ti3C2T x Serious loss of membrane material occurs.
[0015] The above-mentioned three-dimensional porous Ti3C2T x The method for preparing a membrane material is characterized in that the stirring time in step 1 is 0.25h to 2h.
[0016] The present invention controls the stirring time to ensure that the Ti3C2T x Self-assembly of nanosheets with surfactant F127.
[0017] The above-mentioned three-dimensional porous Ti3C2T x The method for preparing the membrane material is characterized in that the pyrolysis process in step three is: under argon conditions, the temperature is raised to 300°C to 400°C at a rate of 1°C / min to 10°C / min, and the temperature is kept for 0.5 to 3 hours.
[0018] The present invention controls the pyrolysis temperature range and the heat preservation time to ensure that the surfactant F127 is completely decomposed, leaving pores to achieve the construction of a three-dimensional porous structure.
[0019] The present invention also discloses a three-dimensional porous Ti3C2T x The membrane material is characterized in that it is prepared by the above method.
[0020] The above-mentioned three-dimensional porous Ti3C2T xMembrane material, characterized in that the three-dimensional porous Ti3C2T x The pore structure inside the membrane material is interconnected in three dimensions.
[0021] In addition, the present invention also discloses the above three-dimensional porous Ti3C2T x The use of the membrane material is characterized in that the three-dimensional porous Ti3C2T x The membrane material is used as a self-supporting electrode material.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. The present invention uses surfactant F127 as a soft template and adopts a dropwise and stirring method to form Ti3C2T x The nanosheets were mixed with the surfactant F127 and self-assembled, so that the surfactant F127 could be evenly distributed inside the membrane formed after vacuum filtration and drying, thereby making the three-dimensional porous Ti3C2T x The membrane material has a three-dimensional interconnected pore structure, which effectively reduces the Ti3C2T x The nanosheets are stacked and aggregated with each other; the preparation method has a simple process flow, good repeatability, and can be industrialized.
[0024] 2. The present invention sets Ti3C2T x The concentration of nanosheet dispersion solution and surfactant F127 solution and the stirring time are controlled to regulate the three-dimensional porous Ti3C2T x The internal pores of the membrane material enable the controllable construction of the pore structure.
[0025] 3. Three-dimensional porous Ti3C2T prepared by the present invention x The membrane material has sufficient reaction sites, which can improve the electrolyte permeation rate and electron / ion transport efficiency, and has excellent electrochemical performance; at the same time, the three-dimensional porous Ti3C2T x The membrane material also has a certain toughness and can be used as a self-supporting electrode material.
[0026] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The three-dimensional porous Ti3C2T prepared in Example 1 x Microscopic structure of the membrane material magnified 5000 times.
[0028] Figure 2 The three-dimensional porous Ti3C2T prepared in Example 1 x Microscopic structure of the membrane material magnified 60,000 times.
[0029] Figure 3 The three-dimensional porous Ti3C2T prepared in Example 1 x Cyclic voltammograms of membrane materials at different scan rates.
[0030] Figure 4 The three-dimensional porous Ti3C2T prepared in Example 1 x Constant current charge and discharge curves of membrane materials at different current densities.
[0031] Figure 5 The three-dimensional porous Ti3C2T prepared in Example 1 x Membrane material and Ti3C2T prepared in Comparative Example 1 x X-ray diffraction patterns of the films.
[0032] Figure 6 Ti3C2T prepared in Comparative Example 1 x Microscopic structure of the membrane.
[0033] Figure 7 The three-dimensional porous Ti3C2T prepared in Example 1 x Preparation of membrane materials and comparative example 1 Ti3C2T x Cyclic voltammogram of the film at a scan rate of 50 mV / s. DETAILED DESCRIPTION
[0034] Example 1
[0035] The preparation method of this embodiment comprises the following steps:
[0036] Step 1: Add 25 mL of 1 mg / mL Ti3C2T x The nanosheet dispersion solution was added dropwise into 10 mL of a 5 mg / mL surfactant F127 solution and magnetically stirred for 0.5 h to obtain a mixed solution;
[0037] Step 2: vacuum filter the mixed solution obtained in step 1 and form a membrane after drying;
[0038] Step 3: Place the film formed in step 2 in a tube furnace, heat it to 350°C at a rate of 5°C / min under argon atmosphere for pyrolysis for 1 h, and then cool it naturally to obtain a three-dimensional porous Ti3C2T x membrane material.
[0039] The three-dimensional porous Ti3C2T x The membrane material was subjected to mechanical bending test. The three-dimensional porous Ti3C2T x The membrane material can be bent arbitrarily without breaking and can be used as a self-supporting electrode material.
[0040] The three-dimensional porous Ti3C2T prepared in this example x The surface of the membrane material was analyzed by scanning electron microscopy, such as Figure 1 As shown, the three-dimensional porous Ti3C2T x The thickness of the membrane material is about 13 μm. x The internal microstructure of the membrane material is analyzed after it is cut open, such as Figure 2 As shown, the three-dimensional porous Ti3C2T x The membrane material showed an obvious three-dimensional loose structure with a large number of depressions and flocculent protrusions, indicating that the three-dimensional porous Ti3C2T x There are a large number of pores inside the membrane material, and adjacent pores are interconnected.
[0041] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material to conduct cyclic voltammetry curve tests at different scanning speeds, such as Figure 3 As shown in the figure, the cyclic voltammetry curves at different scan rates all show a rectangular shape, and the shape is still rectangular when the scan rate increases to 500 mV / s, indicating that the three-dimensional porous Ti3C2T x The membrane material has high capacitance, excellent ionic response and superior rate capability.
[0042] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material and constant current charge and discharge tests were performed at different scanning speeds, such as Figure 4 As shown in the figure, the constant current charge-discharge curves at different current densities all show a triangular shape, and the shape is still triangular when the current density increases to 30 A / g, indicating that the three-dimensional porous Ti3C2T x The membrane material has high reversibility and excellent Coulombic efficiency.
[0043] After testing, when the current density is 0.5A / g, the three-dimensional porous Ti3C2T x The specific capacitance of the membrane material can reach 272F / g. When the current density is increased to 30A / g, the three-dimensional porous Ti3C2T x The specific capacitance of the membrane material can still be maintained at 61.2% of the specific capacitance at a current density of 0.5 A / g, and the surface three-dimensional porous Ti3C2T x The membrane material has excellent electrochemical properties.
[0044] Comparative Example 1
[0045] The preparation method of this comparative example comprises the following steps: 6 mL of Ti3C2T xThe nanosheet dispersion was diluted with 10 mL of distilled water, and then vacuum filtered and dried to obtain Ti3C2T3 nanosheets with a thickness of about 3 μm. x membrane.
[0046] The Ti3C2T prepared in this comparative example x The three-dimensional porous Ti3C2T prepared in Example 1 x The membrane material was subjected to X-ray diffraction test, such as Figure 5 As shown, the comparative example Ti3C2T x The (002) peak of the film at 7.2° is comparable to that of the three-dimensional porous Ti3C2T x The (002) peak of the film material is narrower and stronger, indicating that the Ti3C2T x The nanosheets produced obvious stacking and aggregation, making the characteristic peaks more obvious.
[0047] The Ti3C2T prepared in this comparative example x The membrane was analyzed by scanning electron microscopy, such as Figure 6 As shown, Ti3C2T x The film shows obvious nanosheet stacking characteristics. x The stacking and aggregation inside the film are obvious, making the Ti3C2T x The film thickness is compared with the three-dimensional porous Ti3C2T x The thinner the membrane material is, the more the three-dimensional porous Ti3C2T x The nanosheets inside the membrane material are stretched by a large number of three-dimensional pores, which significantly increases the thickness of the membrane material.
[0048] The Ti3C2T prepared in this comparative example x The three-dimensional porous Ti3C2T prepared in Example 1 x The membrane materials were used as self-supporting electrode materials in supercapacitors to conduct cyclic voltammetry curve tests at a scan rate of 50 mV / s; Figure 7 As shown, the cyclic voltammetry curve area of this comparative example is significantly smaller than that of Example 1, indicating that the three-dimensional porous Ti3C2T x The membrane material is compared with the Ti3C2T prepared in this comparative example. x Membrane capacitors have better performance.
[0049] Example 2
[0050] The preparation method of this embodiment comprises the following steps:
[0051] Step 1: Add 50 mL of 0.5 mg / mL Ti3C2T xThe nanosheet dispersion solution was added dropwise to 10 mL of a 0.5 mg / mL surfactant F127 solution and magnetically stirred for 0.25 h to obtain a mixed solution;
[0052] Step 2: vacuum filter the mixed solution obtained in step 1, and form a membrane structure after drying;
[0053] Step 3: Place the membrane structure formed in step 2 in a tube furnace, heat it to 300°C at a rate of 1°C / min under argon atmosphere, pyrolyze it for 0.5h, and then cool it naturally to obtain a three-dimensional porous Ti3C2T3 with a thickness of about 10μm. x membrane material.
[0054] The three-dimensional porous Ti3C2T x The membrane material was subjected to mechanical bending test. The three-dimensional porous Ti3C2T x The membrane material can be bent arbitrarily without breaking and can be used as a self-supporting electrode material.
[0055] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material for constant current charge and discharge tests. The specific capacitance reached 112 F / g at a current density of 0.5 A / g. When the current density was increased to 10 A / g, the specific capacitance could still maintain 41% of the specific capacitance at a current density of 0.5 A / g. The surface three-dimensional porous Ti3C2T x The membrane material has excellent electrochemical properties.
[0056] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material for cyclic voltammetry curve testing. When the scan rate increased from 10mV / s to 100mV / s, the cyclic voltammetry curve shape was rectangular, indicating that the three-dimensional porous Ti3C2T x The membrane material has high capacitance, excellent ionic response and superior rate capability.
[0057] Example 3
[0058] The preparation method of this embodiment comprises the following steps:
[0059] Step 1: Add 5 mL of 5 mg / mL Ti3C2T x The nanosheet dispersion solution was added dropwise into 10 mL of a 10 mg / mL surfactant F127 solution and magnetically stirred for 2 h to obtain a mixed solution;
[0060] Step 2: vacuum filter the mixed solution obtained in step 1, and form a membrane structure after drying;
[0061] Step 3: Place the membrane structure formed in step 2 in a tube furnace, heat it to 400°C at a rate of 10°C / min for 3h under argon atmosphere, and then cool it naturally to obtain a three-dimensional porous Ti3C2T3 with a thickness of about 12μm. x membrane material.
[0062] The three-dimensional porous Ti3C2T x The membrane material was subjected to mechanical bending test. The three-dimensional porous Ti3C2T x The membrane material can be bent arbitrarily without breaking and can be used as a self-supporting electrode material.
[0063] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material for constant current charge and discharge tests. The specific capacitance reached 172F / g at a current density of 0.5A / g. When the current density was increased to 20A / g, the specific capacitance could still maintain 45% of the specific capacitance at a current density of 0.5A / g. The surface three-dimensional porous Ti3C2T x The membrane material has excellent electrochemical properties.
[0064] The three-dimensional porous Ti3C2T prepared in this example x The membrane material was used as a self-supporting electrode material for cyclic voltammetry curve testing. When the scan rate increased from 10 mV / s to 200 mV / s, the cyclic voltammetry curve shape was rectangular, indicating that the three-dimensional porous Ti3C2T x The membrane material has high capacitance, excellent ionic response and superior rate capability.
[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A three-dimensional porous Ti3C2T x The method for preparing a membrane material is characterized in that: The preparation method comprises the following steps: Step 1: Ti3C2T x The nanosheet dispersion solution was added dropwise into the surfactant F127 solution and stirred to obtain a mixed solution; Step 2: vacuum filter the mixed solution obtained in step 1 and form a membrane after drying; Step 3: The film formed in step 2 is placed in a tube furnace for pyrolysis, and then cooled naturally to obtain a three-dimensional porous Ti3C2T x membrane material.
2. A three-dimensional porous Ti3C2T according to claim 1 x The method for preparing a membrane material is characterized in that: Ti3C2T x The concentration of the nanosheet dispersion solution is 0.5 mg / mL to 5 mg / mL.
3. A three-dimensional porous Ti3C2T according to claim 1 x The method for preparing a membrane material is characterized in that: The concentration of the surfactant F127 solution in step 1 is 0.5 mg / mL to 10 mg / mL.
4. A three-dimensional porous Ti3C2T3 according to claim 1 x The method for preparing a membrane material is characterized in that: The stirring time in step 1 is 0.25h to 2h.
5. A three-dimensional porous Ti3C2T according to claim 1 x The method for preparing a membrane material is characterized in that: The pyrolysis process in step 3 is: under argon conditions, heating to 300°C to 400°C at a rate of 1°C / min to 10°C / min, and keeping warm for 0.5 to 3h.
6. A three-dimensional porous Ti3C2T x The membrane material is characterized in that The method is prepared by any one of claims 1 to 5.
7. A three-dimensional porous Ti3C2T3 according to claim 6 x The membrane material is characterized in that The three-dimensional porous Ti3C2T x The pore structure inside the membrane material is interconnected in three dimensions.
8. A three-dimensional porous Ti3C2T3 as claimed in claim 6 or 7 x Use of the membrane material, characterized in that The three-dimensional porous Ti3C2T x The membrane material is used as a self-supporting electrode material.
Citation Information
Cited By
In-plane porous Ti3C2Tx sheet and construction method thereof
CN119911907A
Porous Ti3C2Tx material, self-assembly preparation method thereof and application of porous Ti3C2Tx material in supercapacitor
CN120854174A
Method for preparing three-dimensional macroporous Ti3C2TX membrane material by using OP-10 as soft template, membrane material and application of membrane material
CN121171799A