Conductive agent modified electrode material of slurry battery and preparation method of conductive agent modified electrode material
Through the composite modification strategy of active materials and conductive additives, a percolation conductive network is formed, which solves the problems of complex process and high cost of existing lithium slurry batteries, achieves efficient ion-electron transfer and electrochemical performance improvement, and meets the needs of The need for large-scale energy storage.
Patent Information
- Application Number
- CN202410890191.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The existing lithium slurry battery active material modification process is complex and costly, making it difficult to meet the low-cost demand for large-scale energy storage. Moreover, the process flow is long, which reduces production efficiency.
Using a composite modification strategy of active materials and conductive additives, active materials are grown on the conductive additive matrix through solvothermal method to form a conductive carbon layer, which is combined with additional conductive additives to form a percolation conductive network to improve the ion-electron transfer efficiency of the electrode.
It achieves efficient ion-electron transfer at high current density, improves electrochemical performance, simplifies the process, reduces costs, and meets the needs of large-scale energy storage.
Smart Images

Figure CN118782800A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium slurry batteries, and specifically relates to a method for modifying a conductive agent composite active material suitable for high current density and a method for preparing a highly stable slurry. Background Art
[0002] In order to overcome energy problems and promote energy transformation, lithium slurry batteries have attracted widespread attention as a new type of large-scale energy storage technology. Unlike traditional lithium-ion batteries, lithium slurry batteries disperse their commonly used active materials and conductive additives in the electrolyte to form positive and negative electrode slurries, and transmit them to the electrochemical reactor through an external pumping device for electrochemical reactions, thereby realizing energy conversion and storage. Therefore, lithium slurry batteries can decouple energy from power and have huge potential for large-scale energy storage applications. Among them, active materials are an important component of slurry batteries, and their morphology, content, conductivity and other characteristics play an important role in the performance of slurry electrodes. By modifying the active materials, the electron-ion transfer efficiency in the slurry electrode can be effectively improved, the lithium storage capacity can be fully utilized, and a highly stable and high-capacity negative electrode slurry can be constructed. At present, researchers have carried out some research work on active material modification and slurry preparation process optimization.
[0003] CN1113054196A discloses a method for modifying the positive active material of the positive electrode slurry of a lithium slurry battery, first preparing a concentration gradient nickel-cobalt-manganese ternary material, and then grafting it with an ionic liquid after surface modification with a silane coupling agent, and then coating porous graphene. The modification method uses an ionic liquid as a connector to connect the graphene coating layer, ensuring the excellent performance of the active material. However, the process is complicated, the ionic liquid is expensive, and it is difficult to meet the low-cost requirements of large-scale energy storage.
[0004] CN115275157A discloses a negative electrode active material for a lithium slurry battery and a preparation method thereof. A silicon-oxygen material having both carbon coating and carbon-reduced silicon dioxide was prepared by a sol-hydrothermal method and high-temperature heat treatment, and used as a slurry electrode active material. The modification strategy effectively improves the surface bonding force and interface compatibility of the material, while promoting the release of local applied forces to alleviate the volume expansion and particle crushing problems during the silicon charging and discharging process, ensuring the formation of a stable solid electrolyte interface and enhancing the kinetic diffusion of lithium ions. The modification process involves harsh acidic conditions, which introduces additional requirements for equipment; and the process flow is too long, which reduces production efficiency.
[0005] CN110165157B discloses a method for uniformly mixing lithium titanate slurry containing carbon nanotubes, the process comprising adding a binder to an electrolyte to prepare a gel, then adding carbon nanotubes to prepare a conductive gel, and then mixing a mixed dry material formed by a conductive agent and a main ingredient with the conductive gel to prepare lithium titanate slurry containing carbon nanotubes. The preparation method is a preparation strategy for lithium ion battery slurry, and the slurry is fully mixed, which has important guiding significance for the preparation process of lithium slurry electrodes.
[0006] Therefore, a novel lithium slurry electrode active material modification strategy is needed in the art to prepare a slurry electrode with efficient ion-electron transfer, enable it to operate at a high current density, and have good electrochemical performance. At the same time, the preparation process is simple and cost-saving. Summary of the invention
[0007] In view of the shortcomings of the prior art, one of the purposes of the present invention is to provide a novel lithium slurry electrode active material modification strategy, characterized in that the strategy combines the active material with a conductive additive to improve the material conductivity; the uncompounded exposed conductive additive can be dispersed with the active material in the electrolyte to form a percolation conductive network, thereby strengthening the ion-electron transfer inside the electrode. The active material is bronze phase titanium dioxide (TiO2(B)), titanium niobium oxide (TiNb2O7, etc.), lithium titanate (Li4Ti5O 12 ), silicon oxide, silicon dioxide, etc., or a combination of two or more thereof; the conductive agent is conductive carbon black (Surper P), Ketjen black (KB), single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers (CNF), reduced graphene oxide (rGO) and graphene (GO) or a combination of two or more thereof. The electrolyte is composed of a lithium salt and a solvent; the lithium salt is one or a combination of two or more thereof selected from LiPF6, LiTFSI, LiBOB and LiDFOB, and the molar mass concentration thereof in the electrolyte is 1 to 3 mol / L; the solvent is at least one of carbonate, ether and carboxylate.
[0008] The mass proportion of the active material in the slurry is 5% to 55%; the mass proportion of the conductive agent in the slurry is 0% to 2%; the sum of the mass proportions of the active material, the conductive agent and the electrolyte is 100%.
[0009] The modification strategy of the present invention includes but is not limited to the growth of active materials on the conductive additive matrix; the conductive additive covers the active material to form a conductive carbon layer, etc. The active material and the conductive additive are compounded to effectively improve the conductivity of the electrode material; the conductive additive that is not compounded and exposed can form an electrode percolation conductive network together with the additional conductive additive (optional) added during the slurry preparation process, thereby strengthening the ion and electron transfer path inside the electrode and improving the electrochemical performance of the electrode.
[0010] The second object of the present invention is to provide a preparation process of a modified slurry of an active material composite conductive additive, wherein the active material is bronze phase titanium dioxide (TiO2(B). The raw materials used in the present invention are widely available, and the preparation process is simple and easy to control, which is conducive to achieving the production needs of large-scale energy storage. The preparation method comprises the following steps:
[0011] 1. The modification method is a solvent thermal method, in which a conductive additive aqueous solution is added during the solvent reaction heat process.
[0012] 2. Grow titanate composite precursors on the surface of conductive additives through traditional solvothermal reaction.
[0013] 3. Annealing the titanate composite precursor in an inert atmosphere to obtain a bronze phase titanium dioxide composite material.
[0014] 4. The bronze phase titanium dioxide composite material and additional conductive additives are dispersed in the electrolyte by mechanical mixing to construct a negative electrode composite slurry for applications under high current density.
[0015] Preferably, the conductive additive for compounding is one or a combination of two or more of a single-walled carbon nanotube aqueous solution, a reduced graphene oxide aqueous solution, and a graphene oxide aqueous solution, with a mass fraction of 0.1 to 10 wt%, for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%.
[0016] Preferably, the organic solvent of the solvothermal reaction is ethanol, ethylene glycol or glycerol.
[0017] Preferably, the titanium source material is titanium trichloride solution and / or titanium tetrachloride solution.
[0018] Preferably, the titanium trichloride solution, deionized water and the conductive additive aqueous solution are uniformly dissolved in the organic solution to perform a solvothermal reaction.
[0019] Preferably, the volume ratio of the total volume of the conductive additive aqueous solution and deionized water to the titanium trichloride solution is 0.1-1.5, for example, 0.1, 0.2, 0.5, 0.8, 1.0, 1.25 or 1.5.
[0020] Preferably, the volume ratio of the titanium trichloride solution to the organic solution is 1:15 to 2:15, for example, 1:15, 1.5:15 or 2:15.
[0021] Preferably, the dispersion process comprises first mixing a deionized water solution and a conductive additive water solution to obtain a carbon-based solution 1, and then uniformly dispersing the carbon-based solution by any one of ultrasonic and mechanical stirring. The mixing and dispersing time is 1 to 4 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.
[0022] Preferably, the carbon-based solution 1 is dispersed in an organic solvent to obtain a mixed solution 2. The selected mixing method is any one of ultrasonic and mechanical mixing or a combination of multiple methods, and the mixing time is 1 to 4 hours.
[0023] Preferably, the titanium source material solution is added to the organic solvent to obtain a mixed solution 2. The selected mixing method is any one of ultrasonic and mechanical mixing or a combination of multiple methods, and the mixing time is 1 to 4 hours.
[0024] Preferably, the solvent is transferred to a reaction vessel for reaction, ensuring that the filling amount of the inner volume of the vessel is 10-60%, for example, 10%, 20%, 30%, 40%, 50% or 60%.
[0025] Preferably, the solvent thermal reaction process control temperature is 120-180°C, for example, it can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C; the reaction time is 3-24h, for example, it can be 3h, 6h, 9h, 12h, 15h, 18h, 21h or 24h.
[0026] Preferably, after the solvothermal reaction process is completed and cooled to room temperature, solid 1 is obtained by filtration or centrifugation. The centrifugal rate is 5000-10000 r / min, for example, 5000 r / min, 6000 r / min, 7000 r / min, 7000 r / min, 8000 r / min, 9000 r / min or 10000 r / min, and the centrifugal time is 1-15 min, for example, 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, etc.
[0027] Preferably, the solid 1 is washed with ethanol and water for multiple times, and the solid 2 is obtained by centrifugation or filtration.
[0028] Preferably, the solid 2 is dried to obtain a titanate composite conductive additive precursor, wherein the drying is air-blast drying or vacuum drying.
[0029] Preferably, the drying temperature is 50-80°C, for example, it can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the drying time is 24-72h, for example, it can be 24h, 25h, 26h, 28h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h or 72h, etc.
[0030] Preferably, the titanate precursor is annealed to obtain the active composite material.
[0031] Preferably, the annealing environment is an inert atmosphere, such as a nitrogen atmosphere or an argon atmosphere.
[0032] Preferably, the heating rate of the annealing process is 1-15°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min or 15°C / min.
[0033] Preferably, the annealing process maintains a constant temperature of 200-400°C, for example, 200°C, 250°C, 300°C, 350°C or 400°C.
[0034] Preferably, the annealing process maintains a constant temperature for 10 to 480 min, for example, 10 min, 30 min, 60 min, 120 min, 180 min, 240 min, 300 min, 360 min, 420 min or 480 min.
[0035] Preferably, in step 4, the active composite material and the conductive additive are dispersed into the electrolyte to obtain a negative electrode composite slurry.
[0036] Preferably, the mass fraction of the active composite material is 5-55%, for example, 5%, 15%, 25%, 35%, 45% or 55%.
[0037] Preferably, the mass fraction of the conductive additive is 0.1-2%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8% or 2.0%.
[0038] Preferably, the mixing method is mechanical mixing, ultrasound or the like, or a mixture thereof; the mixing time is 0.5 to 4 h, for example, 0.5 h, 1.0 h, 1.5 h, 2.0 h, 2.5 h, 3.0 h, 3.5 h or 4.0 h.
[0039] The preparation method described in the present invention improves the electrical conductivity and ion conduction of the active material, and gives full play to the electrochemical properties of the material; the composite and additional conductive additives together form a strong and efficient percolation conductive network, reduce the sedimentation rate of the active material in the slurry, fully stabilize the slurry, and form a highly stable slurry electrode; compounding with a highly conductive conductive additive reduces the amount of additional conductive additives while ensuring the conductivity of the slurry, and correspondingly increases the limit of the active material load in the slurry electrode, further meeting the volume capacity requirements of large-scale energy storage.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) The modification strategy of active material composite conductive additives adopted in the present invention can ensure the formation of an efficient percolation conductive network inside the slurry electrode on the basis of improving the conductivity of the electrode material. At the same time, it can accelerate the diffusion of lithium ions inside the slurry electrode, improve the interface electrochemical reaction kinetics, and give full play to the electrochemical performance of the active material.
[0042] (2) The modification strategy of the present invention allows for more complete contact between the active material and the conductive additive, alleviates active material sedimentation, and significantly improves slurry stability. On the basis of ensuring sufficient electron conduction paths, the amount of additional conductive additives added to the slurry can be reduced, and accordingly the loading amount of the active material can be increased, thereby increasing the volume energy density of the slurry and meeting large-scale energy storage needs.
[0043] (3) The improved process of the present invention is to introduce a conductive additive during the solvent thermal synthesis of the material, which is simple and has high operational feasibility. At the same time, the process conditions are mild and the process is easy to control, meeting the needs of large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a schematic diagram of the negative electrode slurry configured with the active composite material proposed in the present invention.
[0045] Figure 2 This is a SEM image of the active composite material prepared in specific example 1 of the present invention.
[0046] Figure 3 This is a TEM image of the active composite material prepared in specific example 1 of the present invention.
[0047] Figure 4 It is the BET diagram of the active composite material prepared in specific example 1 of the present invention.
[0048] Figure 5 is the yield stress of the active composite material prepared in specific embodiment 1 of the present invention.
[0049] Figure 6 This is an electrochemical performance diagram of the active composite material configuration slurry prepared in specific embodiment 1 of the present invention. DETAILED DESCRIPTION
[0050] In order to elaborate the present invention and facilitate the reader to understand its application, the following specific examples are listed as an exemplary illustration of the present invention. It should be understood by those skilled in the art that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0051] Example 1
[0052] An active material composite conductive additive slurry (schematic diagram thereof) Figure 1 ), the preparation method is carried out at room temperature, and the process is as follows:
[0053] (1) Mix 1 mL of single-walled carbon nanotube solution (mass fraction of 0.2 wt%) and 1 mL of deionized water solution, and ultrasonicate for 2 h. Add the mixed solution dropwise into 30 mL of ethylene glycol solution and stir for 2 h to obtain mixed solution 1. Add 2 mL of titanium trichloride solution dropwise into mixed solution 1 and stir for 2 h to obtain mixed solution 2. Transfer the mixed solution 2 to a 100 mL reactor and place it in a 150 ° C blast oven for reaction for 6 h. After the reaction is completed and cooled to room temperature, select a speed of 8000 r / min for centrifugation, and the single centrifugation time is 10 min. Wash with ethanol and water several times in turn, and centrifuge to obtain a gray-black solid mixture. Place it in a vacuum oven at 60 ° C and dry it for 12 h to obtain a titanate composite carbon nanotube precursor.
[0054] (2) Anneal the titanate composite precursor obtained in step 1 in a tube furnace in an atmosphere of high-purity argon. The annealing heating rate is 3°C / min and the temperature is raised to 350°C. The annealing process is maintained at 350°C for 0.5h and then cooled naturally to room temperature. The annealed solid is fully ground to obtain an active composite material A.
[0055] (3) The active composite material A, the conductive additive KB and the electrolyte were prepared into a slurry at a mass ratio of 15:1:84. First, KB was added to the electrolyte and mixed for 2 h using a planetary mixer to obtain a mixed suspension 1. Then, the active composite material A was added in proportion and mixed for 2 h using a planetary mixer to obtain an active composite material slurry.
[0056] The SEM image of the active composite material prepared in this example is as follows: Figure 2As shown, from Figure 2 It can be seen that the nano-active material grows along the single-walled carbon nanotubes, the CNTs are dispersed relatively evenly, and the material morphology is diverse, including uniform nano-flower structures, nano-rod-like structures growing along the single-walled carbon nanotubes, and bare carbon nanotubes that are not coated with nano-active materials; its TEM image is shown in Figure 3 As shown, from Figure 3 It can be further verified that the nano-active materials and carbon nanotubes form a good composite, rather than a simple mechanical mixing effect; Figure 4 This is the BET diagram of the active composite material of this example. The results show that after composite modification, the specific surface area of the material is significantly improved, and the contact between the active composite material and the electrolyte is more sufficient. Figure 5 The medium shear rheological behavior shows that the composite modification significantly increases the yield stress of the slurry and significantly improves the stability of the slurry.
[0057] Example 2
[0058] The difference from Example 1 is that the conductive additive solution in step (1) is a reduced graphene oxide solution (mass fraction is 0.2wt%) and the volume is 1mL.
[0059] Example 3
[0060] The difference from Example 1 is that the conductive additive solution in step (1) is 0.5 mL of reduced graphene oxide solution (mass fraction is 0.2 wt%) and 0.5 mL of single-walled carbon nanotube solution (mass fraction is 0.2 wt%).
[0061] Example 4
[0062] The difference from Example 1 is that the conductive additive in step (3) is reduced graphene oxide.
[0063] Example 5
[0064] The difference from Example 1 is that the conductive additive in step (3) is carbon nanofiber.
[0065] Example 6
[0066] The difference from Example 1 is that no additional conductive additive is added in step (3). The mass percentage of the active composite material and the electrolyte in the slurry is 25:75.
[0067] Comparative Example 1
[0068] The difference from Example 1 is that in step (1), the single-walled carbon nanotube solution is 0 mL and the deionized water is 2 mL.
[0069] Comparative Example 2
[0070] The difference from Example 1 is that the active material in step (3) is the sample obtained in Comparative Example 1, and the conductive additive is single-walled carbon nanotubes.
[0071] Comparative Example 3
[0072] The difference from Example 1 is that the annealing process in step (2) is maintained at a constant temperature of 300°C.
[0073] Comparative Example 4
[0074] The difference from Example 1 is that in step (3), the mass fraction of the active composite material is 5%, the mass fraction of the conductive additive is 1%, and the mass fraction of the electrolyte is 89%.
[0075] The prepared active composite material slurry was subjected to the following electrochemical performance tests:
[0076] (1) Assembly of lithium slurry battery: Cut the conductive carbon cloth into discs with a diameter of 14 mm and use them as the load of the slurry electrode. Evenly coat the prepared slurry on the carbon cloth and weigh it to ensure that the loading amount of active material is between 1.5 and 2 g / cm 2 , and then assembled into a button cell with Celgard2325 diaphragm (16mm diameter) and lithium sheet (15.8mm diameter, 0.5mm thickness). The assembly of lithium slurry reactor battery is similar to that of button cell, and the size of carbon cloth and diaphragm needs to be designed according to the flow channel of the reactor. Make sure that all assembly processes are carried out in a glove box filled with argon.
[0077] (2) Energy density test: A battery tester was used to perform constant current charge and discharge tests, with a charge cut-off voltage of 3.0 V and a discharge cut-off voltage of 1.0 V. After the battery was activated at 0.01C for two cycles, the battery's cycle performance and coulombic efficiency were tested at a current density of 0.5C. The battery was cycled 100 times at 0.5C, and the capacity decay rate of each cycle was calculated. The high current density cycle was run at a current density of 2C.
[0078] Table 1
[0079]
[0080] It can be seen from Table 1 that, compared with Comparative Example 1, when tested at a current density of 0.5C, the cycle specific capacity and coulombic efficiency of the slurry electrode of Examples 1 to 5 are reduced, and the capacity decay rate is reduced, indicating that the composite modification significantly improves the cycle stability of the slurry and the electrochemical performance is more excellent. At a current density of 2C, Example 1 can still have 173.7 mAh g after 500 cycles. -1 The capacity retention rate is 78.8% (such as Figure 6). This can be attributed to the significant improvement in the conductivity of the active material when composited with the highly conductive material.
[0081] It can be seen from Table 1 that at a current density of 0.5C, Example 3 exhibits a higher specific capacity and cycle stability than Examples 1 to 2. The performance of the active material composited with two-dimensional conductive additives (reduced graphene oxide and single-walled carbon nanotubes) is higher than that of the composite modification with a single-dimensional conductive agent. This can be attributed to the fact that the multi-dimensional conductive agent makes full use of the synergistic effect between conductors of different dimensions to form a multi-dimensional conductive network, which complements each other, allowing the conductive agent and the active material to fully contact, thereby improving the conductive efficiency. The multi-dimensional conductive agent is more conducive to the uniform growth of the active material on the conductive agent, giving full play to the lithium storage capacity of the material.
[0082] It can be seen from Table 1 that, compared with Example 1, at a current density of 0.5C, the cycle capacity, coulombic efficiency and stability of the slurry in Examples 4 to 5 are all reduced, indicating that when the additional conductive additives are at the same content, the influence of their morphology on the slurry performance cannot be ignored. When additional conductive additives with different morphologies are introduced, the percolation threshold of the slurry changes, which needs to be further determined.
[0083] It can be seen from Table 1 that the cycle specific capacity and stability of Example 6 at a current density of 0.5C are both lower than those of Example 1. No additional conductive additives are added to the slurry of Example 6, and accordingly, the mass percentage of the active composite material is increased to 25%. Although a part of the capacity is lost, the effect of increasing the active material loading in the slurry is significant, which has great practical value.
[0084] It can be seen from Table 1 that the cycle specific capacity and capacity attenuation rate of the slurry of Comparative Examples 1 to 2 are both lower than those of Example 1 at a current density of 0.5C. This shows that the composite modification of the active material using a conductive agent is different from the simple mechanical mixing during the slurry preparation process. The composite modified conductive additive and the conductor improve the conductivity of the material, and as an important part of the percolation conductive network in the slurry, provide an efficient and strong electronic conduction path.
[0085] It can be seen from Table 1 that, compared with Example 1, at a current density of 0.5C, the specific capacity and cycle stability of the slurry in Comparative Example 3 are reduced, indicating that optimizing the synthesis process parameters of the active material has an important influence on improving the performance of the material.
[0086] It can be seen from Table 1 that the cycle specific capacity and stability of the slurry of Comparative Example 4 are lower than those of Example 6 at a current density of 0.5C, indicating that the content of active substances in the slurry is reduced, so that an interconnected conductive network cannot be formed inside the slurry, the utilization rate of active materials is lower, and the electrochemical performance is limited. The content and morphology of active substances and conductive agents in the slurry significantly affect the slurry performance, and further optimization is required for the development of the slurry.
[0087] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for modifying conductive composite active materials and a process for preparing highly stable slurry, characterized in that: The preparation method comprises: (1) growing a precursor on the surface of a single-walled carbon nanotube conductive agent by a conventional solvothermal reaction, wherein the solvothermal reaction is carried out at 150° C. for 6 hours; (2) drying the precursor in step (1) and annealing it in an inert atmosphere to obtain an active composite material, wherein the annealing process is carried out in a tubular furnace filled with argon gas, with a heating rate of 3° C. / min, a controlled temperature of 350° C., and a holding time of 30 minutes; (3) The active composite material of step (2) and the conductive additive are dispersed in the electrolyte by mechanical mixing to prepare a composite slurry that operates at a high current density.
2. The preparation method according to claim 1, characterized in that: Conductive agents are added to modify active materials during the traditional solvothermal reaction process to synthesize active composite materials; The conductive agent is one or a combination of two or more selected from conductive carbon black (Surper P), Ketjen black (KB), single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers (CNF), reduced graphene oxide (rGO) and graphene (GO), preferably one or a combination of two or more selected from Ketjen black (KB) and single-walled carbon nanotubes (SWCNT); The active material is bronze phase titanium dioxide (TiO2(B)), titanium niobium oxide (TiNb2O7, etc.), lithium titanate (Li4Ti5O 12 ), silicon oxide, silicon monoxide, etc. or a combination of two or more thereof.
3. The preparation method according to claim 1, characterized in that: In the traditional solvothermal reaction process, ethylene glycol is used as a solvent, and titanium trichloride solution, single-walled carbon nanotube aqueous solution and deionized water are added; it is ensured that the total volume ratio of deionized water and single-walled carbon nanotube aqueous solution to the volume ratio of titanium trichloride solution is 1:1, and the volume ratio of titanium trichloride solution to ethylene glycol solution is 1:
15.
4. The preparation method according to claims 1 and 3, characterized in that: The content ratio of adding titanium trichloride solution to single-walled carbon nanotube aqueous solution is 1mL:0-3.75g, and the corresponding content of adding deionized water is 1mL-0mL; Preferably, when the content of the titanium trichloride solution is 1 mL, the contents of deionized water and single-walled carbon nanotubes are 0.25 mL and 0.75 g, respectively.
5. The preparation method according to claims 1-4, characterized in that: The precursor was washed with water and ethanol for several times, and then dried in an oven at 60° C. for 12 hours. After drying, it was annealed in an inert atmosphere to obtain an active particle composite conductive agent material, which was used as an active material for a slurry electrode.
6. A high-capacity titanium dioxide composite carbon nanotube negative electrode material, characterized in that: The negative electrode material comprises various morphologies, and the mass fraction of the composite carbon nanotubes is 1%-5%; Preferably, the composite material morphology includes a regular nanoflower morphology formed by nanosheets, a nanorod-like titanium dioxide structure formed on the surface of carbon nanotubes, and bare carbon nanotubes; Preferably, the compounding amount of the carbon nanotubes is 1%.
7. The preparation method according to claim 1, characterized in that: The electrolyte is a conventional electrolyte for lithium-ion batteries, consisting of lithium salt, additives and solvent; Preferably, the electrolyte solvent is a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) in a mass ratio of 3:7; Preferably, the lithium salt in the electrolyte is lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) with a content of 1 mol L -1 .
8. The preparation method according to claims 1-7, characterized in that: uniformly dispersing a titanium dioxide composite carbon nanotube negative electrode material and a conductive additive in an electrolyte by mechanical mixing to obtain a negative electrode slurry; Preferably, the negative electrode material and the conductive additive are ultrasonicated in the electrolyte for 1 hour; Preferably, the mass fractions of the negative electrode material and the conductive additive in the slurry are 15% and 1% respectively; Preferably, the mechanical mixing is carried out in a planetary mixer for a mixing time of 1 hour.
9. A composite slurry electrode suitable for high current density, characterized in that: The negative electrode slurry comprises the titanium dioxide composite carbon nanotube material according to claim 6.
Citation Information
Patent Citations
Preparation method of graphene / titanium dioxide composite photocatalyst
CN101890344A
Preparation method for carbon nano tube loaded anatase nano titanium dioxide
CN104549203A
Composite positive electrode material, preparation method thereof and lithium ion battery
CN112216829A
Battery slurry as well as preparation method and application thereof
CN115566194A
Magnetically modified semi-solid fluid negative electrode and preparation method and application thereof
CN115986134A