Composition, preparation method and application of composition in all-vanadium redox flow battery
By using a combination of catalyst Cr2O3, MoO2 and foamed carbon, the electrode structure is optimized to solve the problems of electrode felt thickness, fiber penetration and pore structure in all-vanadium redox flow batteries, thereby improving battery performance and durability.
Patent Information
- Application Number
- CN202410949721.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-15
AI Technical Summary
The all-vanadium redox flow battery has an electrode felt body that is too thick, longitudinal carbon fibers puncture the membrane, and a constant pore structure that is not conducive to the uniform distribution of chemically active substances and unstable activation effects, resulting in poor electrochemical performance and durability.
Using a combination of catalyst Cr2O3, MoO2 and foamed carbon, through needle punching compounding, carbonization, graphitization treatment and catalyst activation foaming, an electrode felt with excellent conductivity and reasonable pore size distribution is prepared, combined with multi-body density pre-oxidized silk fiber Optimize electrode structure.
It improves the electrochemical performance and durability of the battery, enhances the catalytic activity and conductivity of the electrode, reduces the polarization and pump loss of the battery, and extends the cycle life of the electrochemical performance.
Smart Images

Figure CN118782811A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of electrochemical energy storage technology, and in particular relates to a composition, a preparation method and an application thereof in an all-vanadium liquid flow battery. Background Art
[0002] In recent years, with the massive consumption of fossil energy and the intensification of environmental pollution, the widespread use of renewable energy has become increasingly important. Among various electrochemical energy storage technologies, all-vanadium liquid flow batteries are one of the preferred technologies for large-scale energy storage due to their high safety, long life, high efficiency, and environmental friendliness. Among them, the stack is the main core component of the all-vanadium liquid flow battery system, and its power body density determines the cost of the stack. The higher the power body density, the smaller the stack volume and the lower the cost under the same output power conditions. The stack is the core technical component of the liquid flow battery, providing a place for chemical reactions for the positive and negative electrolytes of the liquid flow battery; the stack structure of the liquid flow battery consists of the following five parts: ion exchange membrane, electrode, bipolar plate, current collector and end plate, among which the diaphragm and electrode are the core materials in the stack. As one of the key materials of the all-vanadium liquid flow battery, the thinning, low flow resistance, and high uniform distribution flow channel structural design of the electrode material is an important development trend today and in the future.
[0003] In the prior art, all-vanadium liquid flow batteries have the following technical defects: First, the electrode felt is too thick (2.5-6mm), resulting in a longer electrolyte liquid flow path in the battery stack, affecting the power density and power storage capacity of the battery; Second, very fine longitudinal carbon fibers are distributed on the surface of the electrode, which can easily pierce the membrane and cause internal leakage in the battery stack. The contact resistance between the electrode and the membrane is too large, affecting the performance of the battery stack; Third, most electrodes are porous structures with constant pores, which is not conducive to the uniform distribution of chemically active substances. The concentration of chemically active substances is highest at the interface between the electrode and the bipolar plate, and is lower near the ion exchange membrane side, resulting in a decrease in the overall utilization rate of the electrode material and easily causing polarization of the battery; Fourth, the activation effect of the electrode felt is unstable, and the activation durability needs to be improved. After hundreds of cycle tests, the electrochemical performance decays significantly.
[0004] Therefore, developing a composition, a preparation method and its application in all-vanadium liquid flow batteries to solve the technical defects of the prior art, namely, poor electrochemical performance and durability of all-vanadium liquid flow batteries, has become an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] Based on this, it is necessary to provide a composition, a preparation method and its application in all-vanadium liquid flow batteries to address the technical defects of the existing technology, such as poor electrochemical performance and durability of all-vanadium liquid flow batteries.
[0006] The present application provides a composition, the raw materials of which include: a catalyst, a dispersant, a solvent, a foaming agent and a foam stabilizer;
[0007] The catalyst is selected from any one or more of Cr2O3, MoO2 and foamed carbon.
[0008] In one embodiment, the catalyst includes: 0.1-2 parts of Cr2O3, 0.1-2 parts of MoO2 and 1-5 parts of foamed carbon.
[0009] In one embodiment, the raw materials of the composition include, by weight: 2 to 10 parts of a catalyst, 5 to 10 parts of a dispersant, 80 to 90 parts of a solvent, 1 to 5 parts of a foaming agent, and 0.3 to 1 part of a foam stabilizer.
[0010] In one embodiment, the dispersant is selected from any one or more of alkylphenol polyoxyethylene polyoxypropylene ether APEP-108, sodium salt coating dispersant-5040, Triton X-100 and anhydrous ethanol.
[0011] In one embodiment, the foaming agent is selected from: any one or more of an organic foaming agent, an inorganic foaming agent and a microsphere foaming agent;
[0012] and / or,
[0013] The foam stabilizer includes: BYK-8020 and / or BYK-8070.
[0014] The present application also provides a method for preparing an electrode felt using any of the above compositions, the preparation method comprising:
[0015] Step 1, needle punching and compounding: a preoxidized silk fiber preform is needle punched and compounded to obtain a three-dimensional composite needle punched felt, wherein the preoxidized silk fiber preform is composed of a plurality of preoxidized silk fibers with different body densities;
[0016] Step 2: Carbonization and graphitization treatment: the composite needle felt is subjected to carbonization treatment and graphitization treatment in sequence to obtain an intermediate product;
[0017] Step 3: Catalyst activation and foaming: After the catalyst, dispersant and solvent are mixed, stirred and dispersed, a foaming agent and a foam stabilizer are added, stirred and sheared to obtain a catalyst foam liquid;
[0018] Step 4: coating: coating the catalyst foam liquid on the surface of the intermediate product, and obtaining an electrode felt product after low-temperature drying.
[0019] In one embodiment, in step 1, the difference in bulk density of the preoxidized fiber preforms of adjacent bulk density specifications is 0.02 to 0.03;
[0020] In step 1, the thickness of the composite needle felt is 0.5-1.5 mm, and the weight of the composite needle felt is 100-300 g / m 2 .
[0021] In one embodiment, in step 1, the bulk density of the preoxidized silk fiber preform is 0.05±0.01 g / cm 3 , 0.07±0.01g / cm 3 , 0.10±0.01g / cm 3 ;
[0022] In step 1, the bulk density of the composite needle felt is 0.08±0.01 g / cm 3 , 0.1±0.01g / cm 3 , 0.13±0.01g / cm 3 .
[0023] In one embodiment, in step 2, the temperature of the carbonization treatment is 400-1200°C, and the temperature of the graphitization treatment is 1500-2000°C.
[0024] In one embodiment, in step 4, the coating thickness of the catalyst foam liquid is 20-50 mm; the thickness of the electrode felt product is 0.5-1.5 mm, and the gram weight of the electrode felt product is 80-200 g / m 2 .
[0025] In one embodiment, in step 4, the catalyst is coated by one or more of a scraper type, a slit type and a roller type.
[0026] The present application also provides an application of a composition comprising any one of the above or a product obtained by any one of the above preparation methods in an all-vanadium liquid flow battery.
[0027] In summary, the present application provides a composition, including: a catalyst, a dispersant, a solvent, a foaming agent and a foam stabilizer; the catalyst is selected from: any one or more of Cr2O3, MoO2 and foam carbon. The present application also provides a method for preparing an electrode felt using the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in an all-vanadium liquid flow battery. In the technical scheme provided in the present application, the battery performance can be effectively improved by the selection of catalysts; at the same time, a variety of pre-oxidized silk fibers with different body densities can further optimize the conductive properties of the electrode felt; experimental measurements show that the prepared battery has good electrochemical properties, which are better than the control product. The composition, preparation method and application thereof in an all-vanadium liquid flow battery provided in the present application solve the technical defects of the prior art, that is, the all-vanadium liquid flow battery has poor electrochemical performance and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0029] Figure 1 A schematic diagram of a process for preparing electrode felt in the technical solution provided in an embodiment of the present application. DETAILED DESCRIPTION
[0030] The embodiments of the present application provide a composition, a preparation method and application thereof in an all-vanadium liquid flow battery, which are used to solve the technical defects of the prior art, namely, poor electrochemical performance and durability of all-vanadium liquid flow batteries.
[0031] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings and examples. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0032] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0033] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0034] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0035] In the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0036] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0037] Please see below Figure 1 , the protection scheme of the present application will be specifically described in combination with embodiments and comparative examples.
[0038] Example 1
[0039] 1.1 Acupuncture compound
[0040] After the pretreatment of opening, combing and laying, the obtained bulk density is 0.05g / cm 3 , 0.07g / cm 3 , 0.1g / cm 3 The pre-oxidized silk fiber preform is compounded by needle punching to obtain a three-dimensional composite needle punched felt 1; wherein, after the needle punching treatment, the bulk density of the pre-oxidized silk fiber will increase, and the bulk density is 0.08g / cm 3 , 0.1g / cm 3 , 0.13g / cm 3 The thickness of the composite needle-punched felt 1 obtained by needle-punching is 1.35 mm and the weight is 210 g / m 2 .
[0041] 1.2 Carbonization and graphitization treatment
[0042] The composite needle punched felt 1 is sequentially subjected to carbonization treatment and graphitization treatment to obtain an intermediate product 1; the method of carbonization treatment and graphitization treatment is as follows: the composite needle punched felt 1 passes through the carbonization area and the graphitization area sequentially at a speed of 0.6 m / min, the carbonization treatment temperature of the carbonization area is 1000° C., and the graphitization temperature of the graphitization treatment is 2000° C.
[0043] 1.3 Catalyst activation foaming
[0044] 1kgCr2O3, 1kgMoO2, 2kg foamed carbon, 8kg dispersant and 88kg solvent were mixed, stirred and dispersed in a grinding device at 25°C and 800r / min for 2h, and then 3kg foaming agent and 0.5kg foam stabilizer were added. After stirring and shearing in a high-speed stirring and shearing foamer at 25°C and 100r / min for 0.2h, catalyst foam liquid 1 was obtained. In this embodiment, the dispersant is APEP-108, the solvent is deionized water, the foaming agent is AC foaming agent, and the foam stabilizer is BYK-8020 foam stabilizer.
[0045] 1.4 Coating
[0046] The catalyst foam liquid 1 is coated on the surface of the intermediate product 1 by a scraper coating method, and the electrode felt product 1 is obtained after low-temperature drying; wherein the coating thickness of the catalyst foam liquid 1 is 0.07 mm, the thickness of the electrode felt product 1 after drying is 1.31 mm, and the gram weight of the electrode felt product 1 after drying is 141 g / m 2 .
[0047] Example 2
[0048] 2.1 Acupuncture compound
[0049] After the pretreatment of opening, combing and laying, the obtained bulk density is 0.04g / cm 3 , 0.06g / cm 3 , 0.08g / cm 3 The pre-oxidized silk fiber preform is compounded by needle punching to obtain a three-dimensional composite needle punched felt 2; wherein, after the needle punching treatment, the bulk density of the pre-oxidized silk fiber will increase, and the bulk density is 0.06g / cm 3 , 0.085g / cm 3 , 0.10g / cm 3 The thickness of the composite needle-punched felt 2 obtained by needle punching is 1.1 mm and the weight is 161 g / m 2 .
[0050] 2.2 Carbonization and graphitization treatment
[0051] The composite needle punched felt 2 is sequentially subjected to carbonization treatment and graphitization treatment to obtain an intermediate product 2; the method of carbonization treatment and graphitization treatment is as follows: the composite needle punched felt 2 passes through the carbonization area and the graphitization area sequentially at a speed of 0.6 m / min, the carbonization treatment temperature of the carbonization area is 1000°C, and the graphitization temperature of the graphitization treatment is 2000°C.
[0052] 2.3 Catalyst activation foaming
[0053] 1kgCr2O3, 1kgMoO2, 2kg foamed carbon, 8kg dispersant and 88kg solvent were mixed, stirred and dispersed in a ball mill at 25°C and 800r / min for 2h, and then 3kg foaming agent and 0.5kg foam stabilizer were added. After stirring and shearing in a high-speed stirring and shearing foamer at 25°C and 100r / min for 0.1h, catalyst foam liquid 2 was obtained. In this embodiment, the dispersant is 5040, the solvent is deionized water, the foaming agent is AC foaming agent, and the foam stabilizer is BYK-8070.
[0054] 2.4 Coating
[0055] The catalyst foam liquid 2 is coated on the surface of the intermediate product 2 by scraping, and the electrode felt product 2 is obtained after low-temperature drying; wherein the coating thickness of the catalyst foam liquid 2 is 0.1 mm, the thickness of the electrode felt product 2 after drying is 0.88 mm, and the gram weight of the electrode felt product 2 after drying is 105 g / m 2 .
[0056] Example 3
[0057] 3.1 Acupuncture compound
[0058] After the pretreatment of opening, combing and laying, the obtained bulk density is 0.05g / cm 3 , 0.07g / cm 3 , 0.10g / cm 3 The pre-oxidized silk fiber preform is compounded by needle punching to obtain a three-dimensional composite needle punched felt 3; wherein, after the needle punching treatment, the bulk density of the pre-oxidized silk fiber will increase, and the bulk density is 0.08g / cm 3 , 0.1g / cm 3 , 0.13g / cm 3 The thickness of the composite needle-punched felt 3 obtained by needle-punching is 1.35 mm and the weight is 210 g / m 2 .
[0059] 3.2 Carbonization and graphitization treatment
[0060] The composite needle punched felt 3 is sequentially subjected to carbonization treatment and graphitization treatment to obtain an intermediate product 3; the method of carbonization treatment and graphitization treatment is as follows: the composite needle punched felt 3 passes through the carbonization area and the graphitization area sequentially at a speed of 0.6 m / min, the carbonization treatment temperature of the carbonization area is 1000°C, and the graphitization temperature of the graphitization treatment is 2000°C.
[0061] 3.3 Catalyst activation foaming
[0062] 2kgCr2O3, 2kgMoO2, 2.5kg foamed carbon, 10kg dispersant and 83.5kg solvent were mixed, stirred and dispersed in a ball mill at 25°C and 800r / min for 2h, and then 3.5kg foaming agent and 0.8kg foam stabilizer were added. After stirring and shearing in a high-speed stirring and shearing foamer at 25°C and 100r / min for 0.2h, catalyst foam liquid 3 was obtained. In this embodiment, the dispersant is APEP-108, the solvent is deionized water, the foaming agent is AC foaming agent, and the foam stabilizer is BYK-8020.
[0063] 3.4 Coating
[0064] The catalyst foam liquid 3 is coated on the surface of the intermediate product 3 by scraping, and the electrode felt product 3 is obtained after low-temperature drying; wherein the coating thickness of the catalyst foam liquid 3 is 0.07 mm, the thickness of the electrode felt product 3 after drying is 1.37 mm, and the gram weight of the electrode felt product 3 after drying is 142 g / m 2 .
[0065] Comparative Example 1
[0066] (1) Preparation of gradient pore pre-oxidized felt by needle punching
[0067] The needle-punched composite felt with a three-dimensional structure is prepared by the steps of opening, carding, laying, and needle-punching. The obtained needle-punched composite pre-oxidized felt has a thickness of 1.35 mm and a gram weight of 210 g / m 2 .
[0068] (2) Carbonization and graphitization treatment
[0069] The needle-punched composite felt prepared in step (1) is subjected to low-temperature carbonization and high-temperature graphitization to prepare graphite felt; wherein the carbonization treatment temperature is 1000°C, the graphitization treatment temperature is 2000°C, and the running speed through the carbonization treatment area and the graphitization treatment area is 0.6m / min.
[0070] (3) Air activation treatment
[0071] With the aid of a continuous modification furnace, the graphite felt prepared in step (2) was operated in the furnace under air atmosphere conditions, with a flow rate of 800 L / h and a speed of 0.5 m / min, to obtain reference product 1.
[0072] Comparative Example 2
[0073] (1) Preparation of gradient pore pre-oxidized felt by needle punching
[0074] The needle-punched composite felt with a three-dimensional structure is prepared by the steps of opening, combing, laying, and needle-punching. The thickness of the needle-punched composite pre-oxidized felt is 1.35 mm and the weight is 210 g / m2 .
[0075] (2) Carbonization and graphitization treatment
[0076] The needle-punched composite felt prepared in step (1) was subjected to low-temperature carbonization and high-temperature graphitization to prepare graphite felt. The carbonization treatment temperature was 1000°C, the graphitization treatment temperature was 2000°C, and the running speed through the carbonization treatment area and the graphitization treatment area was 0.6 m / min, thereby obtaining reference product 2.
[0077] Example 4
[0078] This example is an example of measuring the electrochemical properties of electrode felt products 1-3 prepared in Examples 1-3 and reference products 1-2 prepared in Comparative Examples 1-2.
[0079] In this embodiment, the testing methods of various electrochemical properties are as follows:
[0080] Thickness: Use a fabric thickness gauge to test the thickness of the electrode felt without pressure, unit: mm.
[0081] Vertical resistivity: Use a powder resistivity tester to test the resistivity of the electrode felt in the vertical direction under a pressure of 1MPa. Unit: mcm 2 .
[0082] Tensile strength: The tensile strength of the electrode felt is tested using a universal testing machine, unit: MPa.
[0083] Porosity: The porosity of the electrode felt is tested using a true density tester, unit: %.
[0084] Pore size distribution: The mercury intrusion method is used to test the pore size distribution of the electrode felt in the range of 16 to 30 μm, unit: m.
[0085] Coulomb efficiency, energy efficiency, and voltage efficiency tests: Prepare proton membranes, plates, electrodes, peristaltic pumps, vanadium electrolytes, etc. in advance, and use an electrochemical workstation to perform charge and discharge cycle tests on the electrodes. The test temperature is 50°C and the current density is 120 mA / cm 2 .
[0086] In this embodiment, the three major efficiencies are measured after 100 cycles.
[0087] Please refer to Table 1 for the experimental results.
[0088] Table 1
[0089]
[0090]
[0091] It can be concluded from Table 1 that compared with other embodiments, the technical performance parameters of Embodiment 1 are relatively excellent, specifically, its conductivity is good (lowest vertical resistance), the pore size distribution is reasonable, the surface flatness is high (the surface roughness is low), and the three major efficiencies of the battery are high, which can meet the performance requirements of the liquid flow battery.
[0092] In Example 2, the bulk density of the needle-punched preform is adjusted, and the density of the needle-punched composite is appropriately reduced, and finally an electrode felt with lower thickness and gram weight is prepared. Compared with Example 1, the conductivity is similar, the tensile strength is reduced, and the surface flatness is reduced (the thickness consistency control of the low-thickness composite felt is more difficult).
[0093] Compared with Example 1, Example 3 mainly adjusts the catalyst layer formula. The increase in the amount of catalyst filler causes the surface pore size of the electrode felt to shift toward the small pore size, and the target pore size ratio is reduced, which will lead to increased impedance, higher mass transfer losses, and reduced three major efficiencies.
[0094] The higher the vertical resistivity, the worse the conductivity.
[0095] Aperture distribution: A larger proportion of the required pore size range indicates that the pore size is concentrated in a certain range, which is more beneficial to battery performance. The pore size is not the larger the better or the smaller the better, but it can be within a reasonable range.
[0096] The requirement for tensile strength is not high, as long as it does not break under assembly pressure. The higher the value, the better the strength.
[0097] The lower the surface roughness value, the better the surface flatness.
[0098] The higher the above three efficiency values, the better the battery performance.
[0099] The technical solution provided in the embodiment of the present application has the following advantages:
[0100] The electrode felt and preparation method of vanadium flow battery mainly solve the following problems:
[0101] (1) Since the electrode felt of the liquid flow battery in the prior art is too thick (2.5-6mm), the electrolyte liquid flow path in the battery stack will be longer, which not only makes the electrolyte unable to react with the electrode quickly, reducing the redox rate, but also increases the pump loss of the battery, affecting the power density and power storage capacity. The electrode felt prepared by the technical solution provided in the present application has the following advantages: high catalytic activity, excellent conductivity, reasonable mechanical strength and pore size distribution, and high three major efficiencies of the battery.
[0102] (2) In the prior art, very fine longitudinal carbon fibers are distributed on the surface of the electrode, which can easily pierce the membrane and cause internal leakage of the battery stack; the contact resistance between the electrode and the membrane is too large, affecting the performance of the battery stack; the electrode felt prepared by the technical solution provided in the present application has more vertical (Z) fibers inside, which can ensure the excellent conductivity of the electrode felt (electron transmission path segment), small electrolyte flow resistance and uniform flow, and the fibers on the surface of one side of the needle-punched felt (contacting the proton exchange membrane) are distributed in the horizontal (XY) direction, which makes it less likely for upright fibers to pierce the proton exchange membrane.
[0103] (3) In the prior art, most of the electrodes of flow batteries are porous structures with constant pores, which is not conducive to the uniform distribution of chemically active substances, resulting in a decrease in the overall utilization rate of electrode materials and easily causing polarization of the battery; the product prepared by the technical solution provided in this application has a more concentrated pore size distribution near the proton exchange membrane side, and its pore size is smaller than that on the bipolar plate side, and the pore size distribution range near the bipolar plate side is larger. The optimized design of pore size and pore distribution is conducive to further reducing concentration polarization, with large pores serving as transmission channels for electrolytes and small pores serving as active sites for redox reactions.
[0104] (4) The activation effect of the electrode felt in the prior art is unstable, and the activation durability needs to be improved. After hundreds of cycle tests, the electrochemical performance decays significantly. The three major efficiencies in the technical solution provided in this application are measured after 100 cycles, and have better activation durability and smaller attenuation.
[0105] (5) In the catalyst composition provided by the present application, chromium trioxide (Cr2O3) has a low electromotive force, which can improve the reversibility and electrochemical activity of the VO2+ / VO2+ reaction; at the same time, CCr2O3 can inhibit the hydrogen evolution reaction, reduce the overpotential, and improve the voltage efficiency; molybdenum dioxide (MoO2) crystals have a distorted rutile structure, and have the advantages of low resistivity and high stability in acidic solutions; foamed carbon has good conductivity and strong corrosion resistance, and the mesh open pore structure of foamed carbon is conducive to the deposition of active substances therein. After activation, the foamed carbon material has a large specific surface area, and the pore utilization rate can reach 100%, which is conducive to the electrolyte entering the carbon material. In addition, the foamed carbon exhibits good cyclic compression performance under 95% strain, and maintains some elastic properties in the cyclic test, which is suitable for the field of energy storage.
[0106] In summary, the present application provides a composition, including: a catalyst, a dispersant, a solvent, a foaming agent and a foam stabilizer; the catalyst is selected from: any one or more of Cr2O3, MoO2 and foam carbon. The present application also provides a method for preparing an electrode felt using the above composition, and the present application also provides an application of the above composition or the product obtained by the above preparation method in an all-vanadium liquid flow battery. In the technical scheme provided in the present application, the battery performance can be effectively improved by the selection of catalysts; at the same time, a variety of pre-oxidized silk fibers with different body densities can further optimize the conductive properties of the electrode felt; experimental measurements show that the prepared battery has good electrochemical properties, which are better than the control product. The composition, preparation method and application thereof in an all-vanadium liquid flow battery provided in the present application solve the technical defects of the prior art, that is, the all-vanadium liquid flow battery has poor electrochemical performance and durability.
[0107] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. At the same time, other implementation methods can be derived from the above-mentioned embodiments, so that structural and logical replacements and changes can be made without departing from the scope of this disclosure.
[0108] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A composition, characterized in that The raw materials of the composition include: a catalyst, a dispersant, a solvent, a foaming agent and a foam stabilizer; The catalyst is selected from any one or more of Cr2O3, MoO2 and foamed carbon.
2. The composition according to claim 1, characterized in that Calculated by mass, the catalyst includes: 0.1-2 parts of Cr2O3, 0.1-2 parts of MoO2 and 1-5 parts of foamed carbon.
3. The composition according to claim 1 or 2, characterized in that The raw materials of the composition include, by weight, 2 to 10 parts of a catalyst, 5 to 10 parts of a dispersant, 80 to 90 parts of a solvent, 1 to 5 parts of a foaming agent, and 0.3 to 1 part of a foam stabilizer.
4. The composition according to claim 1 or 2, characterized in that The dispersant is selected from any one or more of alkylphenol polyoxyethylene polyoxypropylene ether APEP-108, sodium salt coating dispersant-5040, Triton X-100 and anhydrous ethanol.
5. The composition according to claim 1 or 2, characterized in that The foaming agent is selected from: any one or more of an organic foaming agent, an inorganic foaming agent and a microsphere foaming agent; and / or, The foam stabilizer includes: BYK-8020 and / or BYK-8070.
6. A method for preparing an electrode felt using the composition according to any one of claims 1 to 5, characterized in that: The preparation method is: Step 1, needle punching and compounding: a preoxidized silk fiber preform is needle punched and compounded to obtain a three-dimensional composite needle punched felt, wherein the preoxidized silk fiber preform is composed of a plurality of preoxidized silk fibers with different body densities; Step 2: Carbonization and graphitization treatment: the composite needle felt is subjected to carbonization treatment and graphitization treatment in sequence to obtain an intermediate product; Step 3: Catalyst activation and foaming: After the catalyst, dispersant and solvent are mixed, stirred and dispersed, a foaming agent and a foam stabilizer are added, stirred and sheared to obtain a catalyst foam liquid; Step 4: coating: coating the catalyst foam liquid on the surface of the intermediate product, and obtaining an electrode felt product after low-temperature drying.
7. The preparation method according to claim 6, characterized in that: In step 1, the difference in bulk density of the preoxidized fiber preforms of adjacent bulk density specifications is 0.02 to 0.03; In step 1, the thickness of the composite needle felt is 0.5-1.5 mm, and the weight of the composite needle felt is 100-300 g / m 2 .
8. The preparation method according to claim 6, characterized in that: In step 2, the temperature of the carbonization treatment is 400-1200° C., and the temperature of the graphitization treatment is 1500-2000° C.; In step 2, the composite needle felt passes through the carbonization treatment and graphene treatment area at a speed of 0.1 to 1 m / min.
9. The preparation method according to claim 6, characterized in that: In step 4, the coating thickness of the catalyst foam liquid is 20-50 mm; the thickness of the electrode felt product is 0.5-1.5 mm, and the gram weight of the electrode felt product is 80-200 g / m 2 .
10. Use of the composition according to any one of claims 1 to 5 or the product obtained by the preparation method according to any one of claims 6 to 9 in an all-vanadium redox flow battery.