Modified graphite felt as well as preparation method and application thereof

By combining dodecylbenzenesulfonic acid-doped poly-N-phenylcarbazole with graphite felt, a modified graphite felt is formed, which solves the problems of insufficient conductivity and chemical stability of traditional graphite felt electrodes in vanadium redox flow batteries. , significantly improved the catalytic performance and cycle stability of the battery, extended the life of the electrode, and improved the overall performance of the all-vanadium redox flow battery.

CN118782817APending Publication Date: 2024-10-15SHANXI GEMENG SINO US CLEAN ENERGY R & D CENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410749359.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional graphite felt electrodes have poor conductivity, insufficient chemical stability and low surface activity in vanadium redox flow batteries, which affects the catalytic performance and cycle stability of the battery.

Method used

By combining dodecylbenzene sulfonic acid-doped poly-N-phenylcarbazole with the graphite felt matrix, a modified graphite felt is formed, which improves its conductivity and chemical stability and forms a dense modified layer.

Benefits of technology

It significantly improves the conductivity, charge and discharge efficiency and energy conversion efficiency of the electrode, extends the life of the electrode, improves the corrosion resistance and chemical stability of the battery, and significantly improves the performance of the all-vanadium redox flow battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782817A_ABST
    Figure CN118782817A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of all-vanadium redox flow batteries, and particularly relates to a modified graphite felt as well as a preparation method and application thereof. The invention provides a modified graphite felt. The modified graphite felt comprises a graphite felt matrix and a modified material, the modified material comprises dodecylbenzene sulfonic acid doped poly (N-phenylcarbazole); the modified material is positioned on the surface and inside the graphite felt matrix. The graphite felt is modified through dodecylbenzene sulfonic acid doped with polycarbazole substances, the problems existing in a traditional graphite felt electrode are solved, polycarbazole has good conductivity and chemical stability, a compact modified layer can be formed, the conductivity, the charge-discharge efficiency and the energy conversion efficiency of the electrode are improved, and the electrode has good electrochemical performance. Meanwhile, the corrosion resistance and chemical stability of the battery are improved, and the service life of an electrode is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of all-vanadium liquid flow batteries, and in particular relates to a modified graphite felt and a preparation method and application thereof. Background Art

[0002] As a renewable energy storage system, all-vanadium flow battery has broad application prospects in the fields of grid dispatching, energy storage applications, etc. Its basic structure includes positive and negative electrodes, diaphragms and electrolytes. Graphite felt, as a common electrode material, has been widely used in the field of electrochemical energy, but there are some problems that need to be solved in vanadium flow batteries.

[0003] Traditional graphite felt electrodes have some problems in vanadium flow batteries, including: Low conductivity: Traditional graphite felt electrodes have poor conductivity, which affects the battery's charge and discharge efficiency and performance stability. Poor chemical stability: Traditional graphite felt electrodes are susceptible to corrosion by the electrolyte in vanadium flow batteries, resulting in a short electrode life. Insufficient surface activity: Traditional graphite felt electrodes have low surface activity and limited adsorption capacity for vanadium ions, which is not conducive to the positive electrode VO. 2+ / VO2 + The catalytic activity of the redox reaction of the electrode pair is far less than that of V 2+ / V 3+ Electron pairs affect the catalytic performance and cycle stability of the battery. Summary of the invention

[0004] The object of the present invention is to provide a modified graphite felt and a preparation method and application thereof. The modified graphite felt provided by the present invention is applied to an all-vanadium liquid flow battery to further improve the catalytic performance and cycle stability of the battery.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a modified graphite felt, comprising a graphite felt matrix and a modified material; the modified material comprises dodecylbenzenesulfonic acid-doped poly-N-phenylcarbazole;

[0007] The modified material is located on the surface and inside of the graphite felt matrix.

[0008] Preferably, the doping mass concentration of the dodecylbenzenesulfonic acid in the modified material is 5 to 15%.

[0009] Preferably, the mass percentage of the modified material in the modified graphite felt is 5-20%.

[0010] Preferably, the graphite felt matrix has a purity of 99% and a porosity of 60-90%.

[0011] The present invention also provides a method for preparing the modified graphite felt described in the above technical solution, comprising the following steps:

[0012] mixing dodecylbenzenesulfonic acid, poly-N-phenylcarbazole and an organic solvent to obtain a doping solution;

[0013] The modified graphite felt is obtained by impregnating the graphite felt substrate in the doping solution and then performing a curing treatment.

[0014] Preferably, the organic solvent comprises tetrahydrofuran;

[0015] In the doping solution, the total mass concentration of dodecylbenzenesulfonic acid and poly-N-phenylcarbazole is 5-20%.

[0016] Preferably, the mixing temperature is 25 to 80° C., the mixing is performed under stirring, the stirring speed is 200 to 800 rpm, and the time is 1 to 3 hours.

[0017] Preferably, the doping solution and the graphite felt are used in a ratio of 10 to 200 mL: 1 m 2 ;

[0018] The immersion time is 30 to 180 minutes; the immersion is carried out under stirring, and the stirring speed is 100 to 500 rpm.

[0019] Preferably, the curing treatment is carried out at a temperature of 80 to 100° C. and for a time of 2 to 6 hours.

[0020] The present invention also provides the use of the modified graphite felt described in the above technical solution or the modified graphite felt prepared by the preparation method described in the above technical solution in an all-vanadium liquid flow battery.

[0021] The invention provides a modified graphite felt, comprising a graphite felt matrix and a modified material; the modified material comprises dodecylbenzenesulfonic acid-doped poly-N-phenylcarbazole; the modified material is located on the surface and inside of the graphite felt matrix.

[0022] The invention modifies graphite felt by doping polycarbazole substances with dodecylbenzenesulfonic acid, thereby solving the problems existing in traditional graphite felt electrodes. Polycarbazole has good electrical conductivity and chemical stability, can form a dense modified layer, improves the electrical conductivity, charge and discharge efficiency and energy conversion efficiency of the electrode, and simultaneously improves the corrosion resistance and chemical stability of the battery, thereby prolonging the life of the electrode.

[0023] Compared with traditional graphite felt electrodes, the modified graphite felt of the present invention has the advantages of fast electrochemical reaction rate, long cycle life, strong chemical stability, high mechanical strength, etc., which can effectively improve the performance of all-vanadium liquid flow batteries and has important application value and economic benefits. The modified graphite felt electrode of the present invention can further promote the development of all-vanadium liquid flow battery technology, promote the utilization and storage of clean energy, and promote energy transformation and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The voltage efficiency diagram of the battery assembled with the graphite felts of Examples 1 to 3 and Comparative Examples 1 to 2;

[0025] Figure 2 The capacity efficiency diagram of the battery assembled with the graphite felts of Examples 1 to 3 and Comparative Examples 1 to 2;

[0026] Figure 3 This is a comparison chart of cyclic voltammetry tests of batteries assembled with graphite felt of Example 3 and Comparative Example 1. DETAILED DESCRIPTION

[0027] The present invention provides a modified graphite felt, comprising a graphite felt matrix and a modified material; the modified material comprises dodecylbenzenesulfonic acid-doped poly-N-phenylcarbazole;

[0028] The modified material is located on the surface and inside of the graphite felt matrix.

[0029] In the present invention, the doping mass concentration of the dodecylbenzenesulfonic acid in the modified material is preferably 5 to 15%, and more preferably 8 to 10%.

[0030] In the present invention, the mass percentage of the modified material in the modified graphite felt is preferably 5 to 20%, and more preferably 10 to 15%.

[0031] In the present invention, the purity of the graphite felt matrix is ​​preferably 99%; the porosity is preferably 60-90%, and more preferably 70-80%.

[0032] The present invention also provides a method for preparing the modified graphite felt described in the above technical solution, comprising the following steps:

[0033] mixing dodecylbenzenesulfonic acid, poly-N-phenylcarbazole and an organic solvent to obtain a doping solution;

[0034] The modified graphite felt is obtained by impregnating the graphite felt substrate in the doping solution and then performing a curing treatment.

[0035] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0036] The invention mixes dodecylbenzene sulfonic acid, poly-N-phenylcarbazole and an organic solvent to obtain a doping solution.

[0037] In the present invention, the organic solvent preferably includes tetrahydrofuran. In the present invention, in the doping solution, the total mass concentration of dodecylbenzenesulfonic acid and poly-N-phenylcarbazole is preferably 5-20%.

[0038] In the present invention, the mixing temperature is preferably 25 to 80° C., the mixing is preferably performed under stirring, the stirring speed is preferably 200 to 800 rpm, and the time is preferably 1 to 3 hours.

[0039] In the present invention, the mixing process is preferably: dissolving poly-N-phenylcarbazole in an organic solvent and then adding dodecylbenzenesulfonic acid.

[0040] After obtaining the doping solution, the present invention immerses the graphite felt substrate in the doping solution and then performs a curing treatment to obtain the modified graphite felt.

[0041] Before the impregnation, the present invention also preferably includes pre-treating the graphite felt substrate, and the pre-treatment process is preferably: immersing the graphite felt substrate in an ethanol solution. The present invention has no particular limitation on the specific process of immersion, and any method known to those skilled in the art can be used. In the present invention, impurities on the surface can be removed by immersing in ethanol.

[0042] In the present invention, the dosage ratio of the doping solution to the graphite felt is preferably 10 to 200 mL: 1 m 2 In the present invention, the immersion time is preferably 30 to 180 minutes; the immersion is preferably carried out under stirring, and the stirring speed is preferably 100 to 500 rpm.

[0043] In the present invention, after the impregnation, the impregnated graphite felt is preferably suspended and left to stand until no excess liquid drips.

[0044] In the present invention, the temperature of the curing treatment is preferably 80 to 100° C., and the time is preferably 2 to 6 hours. In the present invention, the curing treatment is preferably performed in an oven.

[0045] After the curing treatment, the present invention also preferably includes post-treatment of the surface of the cured graphite felt; the post-treatment preferably includes: ultrasonic treatment of the cured graphite felt material using deionized water, and the ultrasonic treatment time is preferably 5 minutes. The present invention removes dust and impurities on the surface through ultrasonic treatment.

[0046] The present invention also provides the use of the modified graphite felt described in the above technical solution or the modified graphite felt prepared by the preparation method described in the above technical solution in an all-vanadium redox flow battery. The present invention has no special limitation on the specific manner of the application, and any method known to those skilled in the art can be used.

[0047] In order to further illustrate the present invention, a modified graphite felt provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0048] Example 1

[0049] (1) A graphite felt material with a purity of 99%, a porosity of 80%, and a size of 5×5 cm was selected, and pre-treated by immersion in an ethanol solution to remove surface impurities.

[0050] (2) Dissolve poly (N-phenylcarbazole) PNPCz in tetrahydrofuran solvent, add dodecylbenzenesulfonate (DBS), and stir at 35° C. and 250 rpm for 1.5 h to obtain 20 mL of a doping solution, wherein the ratio of DBS:PNPCz is 5 wt %, and the total mass concentration of the solute in the doping solution is 10%.

[0051] (3) The graphite felt is placed in the doping solution for immersion for 1.5 hours, during which time a stirrer is used for stirring at a speed of 250 rpm. After the immersion is completed, the graphite felt is placed on a bracket until no excess liquid drips from the surface.

[0052] (4) The impregnated graphite felt is placed in an oven for curing, the temperature is set to 100° C., the curing time is 3.5 hours, and the cured graphite felt is ultrasonically treated with deionized water for 5 minutes to obtain the modified graphite felt (the mass percentage of the modified material on the graphite felt is 10%).

[0053] Example 2

[0054] (1) A graphite felt material with a purity of 99%, a porosity of 80%, and a size of 5×5 cm was selected, and pre-treated by immersion in an ethanol solution to remove surface impurities.

[0055] (2) Dissolve poly (N-phenylcarbazole) PNPCz in tetrahydrofuran solvent, add dodecylbenzenesulfonate (DBS), and stir at 35° C. and 250 rpm for 1.5 h to obtain 20 mL of a doping solution, wherein the ratio of DBS:PNPCz is 10 wt %, and the total mass concentration of the solute in the doping solution is 15%.

[0056] (3) The graphite felt is placed in the doping solution for immersion for 1.5 hours, during which time a stirrer is used for stirring at a speed of 250 rpm. After the immersion is completed, the graphite felt is placed on a bracket until no excess liquid drips from the surface.

[0057] (4) The impregnated graphite felt is placed in an oven for curing, the temperature is set to 90° C., the curing time is 3.5 hours, and the cured graphite felt is ultrasonically treated with deionized water for 5 minutes to obtain the modified graphite felt (the mass percentage of the modified material on the graphite felt is 15%).

[0058] Example 3

[0059] (1) A graphite felt material with a purity of 99%, a porosity of 80%, and a size of 5×5 cm was selected, and pre-treated by immersion in an ethanol solution to remove surface impurities.

[0060] (2) Dissolve poly (N-phenylcarbazole) PNPCz in tetrahydrofuran solvent, add dodecylbenzenesulfonate (DBS), and stir at 35° C. and 250 rpm for 1.5 h to obtain 20 mL of a doping solution, wherein the ratio of DBS:PNPCz is 15 wt %, and the total mass concentration of the solute in the doping solution is 20%.

[0061] (3) The graphite felt is placed in the doping solution for immersion for 1.5 hours, during which time a stirrer is used for stirring at a speed of 250 rpm. After the immersion is completed, the graphite felt is placed on a bracket until no excess liquid drips from the surface.

[0062] (4) The impregnated graphite felt is placed in an oven for curing, the temperature is set to 85° C., the curing time is 3.5 hours, and the cured graphite felt is ultrasonically treated with deionized water for 5 minutes to obtain the modified graphite felt (the mass percentage of the modified material on the graphite felt is 20%).

[0063] Comparative Example 1

[0064] A commercially available unmodified graphite felt electrode was selected as a comparative example.

[0065] Comparative Example 2

[0066] The modified graphite felt was prepared in the manner of Example 2, except that the doping operation of dodecylbenzenesulfonic acid was not performed, that is, step (2) was:

[0067] Poly (N-phenylcarbazole) PNPCz was dissolved in tetrahydrofuran solvent, and stirred at 35° C. and 250 rpm for 1.5 h to obtain 20 mL of a doping solution, wherein the total mass concentration of the solute in the doping solution was 20%.

[0068] Performance Testing

[0069] The graphite felts obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were used as electrodes to assemble an all-vanadium liquid flow battery;

[0070] The assembly process is as follows: assemble using a three-electrode system, cut the graphite felt material into 2×2cm using a die knife, use a 3×3cm platinum sheet electrode as the counter electrode, the electrolyte is 0.2M vanadyl sulfate and 3M sulfuric acid, Ag / AgCl is the reference electrode, place the reference electrode in another electrolytic cell filled with potassium chloride solution, and connect with a salt bridge. Connect the assembled battery to the electrochemical workstation for testing.

[0071] The assembled battery was subjected to electrochemical performance testing, wherein the test cycle was 30 cycles;

[0072] Cyclic voltammetry test: set the voltage range to -0.2V~1.5V and the scan rate to 15mV·s -1 .

[0073] The test results are shown in Table 1 and Figures 1 to 3 As shown, Figure 1 Voltage efficiency diagram for battery performance test; Figure 2 Capacity efficiency diagram for battery performance test; Figure 3 This is a comparison chart of cyclic voltammetry tests of batteries assembled with graphite felts of Example 3 and Comparative Example 1;

[0074] Table 1 Performance of batteries assembled from graphite felts of Examples 1 to 3 and Comparative Examples 1 to 2

[0075]

[0076] As can be seen from Table 1, the capacity efficiency and voltage efficiency of the modified graphite felt electrode provided by the present invention are significantly improved, and the peak electric difference also changes significantly and remains stable. After 30 charge and discharge cycle tests, the average reaches 98.7% and 87.3%, which is significantly improved compared with the test of the comparative example.

[0077] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A modified graphite felt, characterized in that: It comprises a graphite felt matrix and a modified material; the modified material comprises dodecylbenzenesulfonic acid-doped poly-N-phenylcarbazole; The modified material is located on the surface and inside of the graphite felt matrix.

2. The modified graphite felt according to claim 1, characterized in that The doping mass concentration of the dodecylbenzenesulfonic acid in the modified material is 5-15%.

3. The modified graphite felt according to claim 1 or 2, characterized in that: The mass percentage of the modified material in the modified graphite felt is 5-20%.

4. The modified graphite felt according to claim 1, characterized in that The purity of the graphite felt matrix is ​​99% and the porosity is 60-90%.

5. The method for preparing the modified graphite felt according to any one of claims 1 to 4, characterized in that: The following steps are involved: mixing dodecylbenzenesulfonic acid, poly-N-phenylcarbazole and an organic solvent to obtain a doping solution; The modified graphite felt is obtained by impregnating the graphite felt substrate in the doping solution and then performing a curing treatment.

6. The preparation method according to claim 5, characterized in that: The organic solvent includes tetrahydrofuran; The total mass concentration of dodecylbenzenesulfonic acid and poly-N-phenylcarbazole in the doping solution is 5-20%.

7. The preparation method according to claim 5, characterized in that: The mixing temperature is 25-80° C., the mixing is performed under stirring, the stirring speed is 200-800 rpm, and the stirring time is 1-3 hours.

8. The preparation method according to claim 5, characterized in that: The dosage ratio of the doping solution to the graphite felt is 10-200 mL: 1 mL 2 ; The immersion time is 30 to 180 minutes; the immersion is carried out under stirring, and the stirring speed is 100 to 500 rpm.

9. The preparation method according to claim 5, characterized in that: The curing treatment is carried out at a temperature of 80 to 100° C. and for a time of 2 to 6 hours.

10. Use of the modified graphite felt according to any one of claims 1 to 4 or the modified graphite felt prepared by the preparation method according to any one of claims 5 to 9 in an all-vanadium liquid flow battery.