Fuel cell metal bipolar plate gradient composite coating and preparation method thereof
By using physical vapor deposition technology combined with metal mesh in fuel cells to prepare nanoarray gradient composite coatings, the problem of corrosion of stainless steel bipolar plates in corrosive environments is solved, the conductivity and corrosion resistance are improved, and the process is simplified and reduce costs.
Patent Information
- Application Number
- CN202310365033.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
AI Technical Summary
In proton exchange membrane fuel cells, stainless steel bipolar plates are prone to corrosion in corrosive environments, resulting in metal ion contamination and reduced conductivity. Traditional physical vapor deposition methods are complex and costly.
Physical vapor deposition technology is combined with metal mesh to prepare a nanoarray gradient composite coating, including a metal gradient layer and an array structure layer, to improve the conductivity and corrosion resistance of bipolar plates without changing the original process plan and reducing process complexity. sex and time costs.
It effectively improves the conductivity and corrosion resistance of the metal bipolar plate, extends the life of the bipolar plate, improves the performance and safety of the fuel cell, simplifies the preparation process, and reduces the complexity of batch processing.
Smart Images

Figure CN118782819A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a gradient composite coating of a metal bipolar plate of a fuel cell and a preparation method thereof. Background Art
[0002] Among various fuel cells, proton exchange membrane fuel cell (PEMFC) is one of the most promising power sources, with the advantages of environmental protection, high efficiency, low operating temperature and near zero emissions. Among the components of PEMFC, bipolar plates play a very important role in PEMFC, providing air flow channels, supporting membrane electrode (MEA) and conducting electricity. However, the bipolar plates in PEMFC must work in an aggressive and corrosive environment. Therefore, the bipolar plates used in PEMFC should have excellent corrosion resistance, high conductivity, reasonable mechanical strength, low cost and good formability.
[0003] Stainless steel is considered to be an ideal material for PEMFC bipolar plates. However, at relatively high ambient temperatures (70-80°C), stainless steel is prone to corrosive dissolution in corrosive electrolytes. The metal ions released after corrosion will contaminate the catalyst and proton exchange membrane, reducing the PEMFC output efficiency. In addition, stainless steel can form a passivation film in a corrosive environment and cause an increase in interfacial contact resistance, which will further reduce the PEMFC conductivity. In order to overcome the shortcomings of stainless steel itself, surface modification technology has been widely used to improve the relevant performance of stainless steel in PEMFC bipolar plates.
[0004] Physical vapor deposition (PVD) is the most commonly used method for preparing coatings on stainless steel. However, traditional PVD solutions require changes to the overall process of the coating, which may affect the comprehensive performance of the coating. There are many limitations in the process of improving process parameters, and multiple modifications may be required, which increases time costs.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide a metal bipolar plate gradient composite coating, which is prepared by combining physical vapor deposition technology with a metal mesh. The metal bipolar plate gradient composite coating has a nanoarray structure, which can effectively improve the conductivity and corrosion resistance of the metal bipolar plate.
[0007] The second object of the present invention is to provide a method for preparing a bipolar plate of a proton exchange membrane fuel cell, wherein the corrosion-resistant conductive coating in the metal bipolar plate can effectively improve the performance of the fuel cell stack.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The present invention provides a metal bipolar plate gradient composite coating, which includes a substrate and a nano-array gradient composite coating;
[0010] The nano-array gradient composite coating comprises a metal gradient layer and an array structure layer, and the array structure layer is obtained by arranging a metal mesh on a substrate and then performing physical vapor deposition.
[0011] Furthermore, the nano-array gradient composite coating also includes a metal gradient layer;
[0012] Preferably, the metal bipolar plate comprises a substrate, a metal gradient layer and an array structure layer in sequence;
[0013] Preferably, the metal bipolar plate comprises a substrate, an array structure layer and a metal gradient layer in sequence.
[0014] Furthermore, the thickness of the nano-array gradient composite coating is 100-250 nm.
[0015] Furthermore, the substrate includes any one of 316L stainless steel, titanium steel or titanium plate.
[0016] Furthermore, the target material for physical vapor deposition includes at least one of a Ti target, a Nb target and a Cr target.
[0017] Furthermore, the metal mesh includes at least one of a stainless steel mesh, a titanium mesh and a copper mesh.
[0018] The present invention provides a method for preparing the above-mentioned metal bipolar plate gradient composite coating, the preparation method comprising the following steps:
[0019] The substrate is ion-etched to obtain an activated surface, and then subjected to physical vapor deposition to obtain a metal gradient layer; a metal mesh is then arranged on top of the metal gradient layer and subjected to physical vapor deposition to obtain a nano-array gradient composite coating;
[0020] Or, a metal mesh is arranged on the substrate and subjected to physical vapor deposition treatment to obtain a metal transition layer having an array structure, and then physical vapor deposition is performed on the metal transition layer to obtain a nano-array gradient composite coating;
[0021] Furthermore, the physical vapor deposition is carried out under high-purity reaction gas;
[0022] Preferably, the high-purity reaction gas includes Ar, C2H2 and N2.
[0023] Furthermore, the preparation method further comprises the step of pretreating the substrate to be treated;
[0024] Preferably, the pretreatment comprises: cutting the substrate to be treated into metal sheets of 50×50 mm in size, then ultrasonically cleaning with acetone, deionized water and anhydrous ethanol for 30 minutes in sequence, and then drying with nitrogen.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention provides a bipolar plate gradient composite coating, which comprises a substrate and a nano-array gradient composite coating deposited on the surface of the substrate. The nano-array gradient composite coating comprises a metal gradient layer and an array structure layer, the metal gradient layer is obtained by activating the substrate surface by strong plasma sputtering and depositing a metal layer, and the array structure layer is obtained by placing a metal mesh above the substrate and then performing physical vapor deposition. The present application adopts physical vapor deposition technology in combination with a metal mesh, and the composite coating of the obtained metal bipolar plate has a nano-array structure, which can effectively improve the conductivity and corrosion resistance of the metal bipolar plate.
[0027] The present invention provides a method for preparing a bipolar plate gradient composite coating. The method can obtain a nano-array gradient composite coating with an array structure by setting a metal mesh above a transition layer and performing a physical vapor deposition treatment, or by directly setting a metal mesh on a substrate to be treated and performing a physical vapor deposition treatment. Therefore, the present application does not need to change the original physical vapor deposition coating preparation process scheme during the preparation process, thereby reducing the complexity and time cost of the process, improving processing efficiency, and facilitating batch processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 A schematic diagram of the preparation principle of the bipolar plate surface array gradient composite coating provided in Example 1 of the present invention;
[0030] Figure 2 A comparison of the surface morphologies of a bipolar plate having an array gradient composite coating on its surface and a 316L stainless steel sheet without a coating provided in Example 1 of the present invention;
[0031] Figure 3 A comparison diagram of contact angle values of a bipolar plate having an array gradient composite coating on its surface and a 316L stainless steel sheet without a coating provided in Example 1 of the present invention;
[0032] Figure 4 This is a comparison diagram of contact angle values of the gradient composite coating on the surface of the bipolar plate of Example 1 of the present invention;
[0033] Figure 5 This is a comparison chart of the corrosion current values of the array gradient composite coating on the surface of the bipolar plate of Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] According to one aspect of the present invention, a metal bipolar plate gradient composite coating comprises a substrate and a nano-array gradient composite coating deposited on a surface of the substrate;
[0036] Among them, the nano-array gradient composite coating includes a metal gradient layer and an array structure layer. The metal gradient layer is obtained by activating the surface of the substrate by strong plasma sputtering and depositing a metal layer, and the array structure layer is obtained by setting a metal mesh above the substrate and then performing physical vapor deposition.
[0037] The present application combines physical vapor deposition technology with a metal mesh, and the composite coating of the prepared metal bipolar plate has a nano-array structure, thereby effectively improving the conductivity and corrosion resistance of the metal bipolar plate.
[0038] In a preferred embodiment of the present invention, the nanoarray gradient composite coating also includes a metal gradient layer; the metal gradient layer can improve the conductivity and corrosion resistance of the coating. At the same time, based on the presence of the metal mesh, the metal gradient layer has better bonding strength with the substrate or the display structure layer, thereby ensuring the good mechanical properties of the metal bipolar plate, extending its life, and ensuring the safety and life of the proton exchange membrane fuel cell.
[0039] Preferably, the metal bipolar plate gradient composite coating comprises a substrate, a metal gradient layer and an array structure layer in sequence;
[0040] Preferably, the metal bipolar plate gradient composite coating comprises a substrate, an exhibition structure layer and a metal gradient layer in sequence.
[0041] In a preferred embodiment of the present invention, the thickness of the nano-array gradient composite coating is 100-250 nm.
[0042] In a preferred embodiment of the present invention, the substrate includes any one of 316L stainless steel, titanium steel or titanium plate.
[0043] In a preferred embodiment of the present invention, the target material for physical vapor deposition includes at least one of a Ti target, a Nb target and a Cr target.
[0044] In a preferred embodiment of the present invention, the metal mesh includes at least one of a stainless steel mesh, a titanium mesh and a copper mesh.
[0045] According to one aspect of the present invention, a method for preparing the above-mentioned metal bipolar plate gradient composite coating comprises the following steps:
[0046] Performing physical vapor deposition on the substrate to be treated to obtain a transition layer; then placing a metal mesh on the transition layer and performing physical vapor deposition to obtain a nano-array gradient composite coating;
[0047] Alternatively, a metal mesh is arranged on the substrate to be treated and subjected to physical vapor deposition treatment to obtain a transition layer having an array structure, and then a physical vapor deposition treatment is performed on the transition layer to obtain a nano-array gradient composite coating;
[0048] The present invention provides a method for preparing a metal bipolar plate, which can obtain a nano-array gradient composite coating with an array structure by arranging a metal mesh above a transition layer and performing a physical vapor deposition treatment, or by directly arranging a metal mesh on a substrate to be treated and performing a physical vapor deposition treatment; therefore, the present application does not need to change the original physical vapor deposition coating preparation process scheme during the preparation process, thereby reducing the complexity and time cost of the process, improving processing efficiency, and facilitating batch processing.
[0049] In a preferred embodiment of the present invention, the physical vapor deposition is carried out under high-purity reaction gas;
[0050] Preferably, the high-purity reaction gas includes C2H2 and N2.
[0051] As a preferred embodiment, during the above-mentioned physical vapor deposition process, a certain proportion of C2H2 or H2 is introduced into the magnetron sputtering chamber, thereby finally obtaining a nano-array structured metal carbide coating with high bonding strength.
[0052] In a preferred embodiment of the present invention, the preparation method further comprises the step of pretreating the substrate to be treated;
[0053] Preferably, the pretreatment comprises: cutting the substrate to be treated into metal sheets of 50×50 mm in size, then ultrasonically cleaning with acetone, deionized water and anhydrous ethanol for 30 minutes in sequence, and then drying with nitrogen.
[0054] Preferably, the method for preparing the metal bipolar plate comprises the following steps:
[0055] (1) The metal substrate was mechanically cut into metal sheets of 50×50 mm in size, and ultrasonically cleaned with acetone, deionized water, and anhydrous ethanol for 30 minutes in sequence, and then dried with nitrogen.
[0056] (2) The cleaned metal substrate was placed on a rotating table in a high-power impulse magnetron sputtering (HiPIMS) furnace to ensure uniformity of coating preparation, and the distance between the target and the sample was kept at 5-20 cm.
[0057] (3) Cover the sample with a layer of 1000-5000 mesh metal mesh with a thickness of 0.1-5 mm and keep the distance between the metal mesh and the sample at 0.1-5 cm.
[0058] (4) Close the chamber, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10 -4 Pa, to keep the furnace in a high vacuum state.
[0059] (5) Fill the furnace with high-purity Ar gas, keep the total pressure constant at 0.1-2 Pa during deposition, and heat the substrate to 0-200°C. After heating, turn on the substrate bias power supply to apply a negative bias of 400-600V, and sputter the substrate surface for 10-30 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0060] (6) Reduce the negative bias voltage of the substrate to 0-100 V, turn on the target current and increase it linearly to 1-5 A within 1-10 min, and maintain it for 10-30 min; maintain the target current and the total working pressure unchanged, and linearly introduce high-purity reaction gas within 1-10 min, with an Ar: reaction gas flow ratio of 10:1-1:1, and maintain it for 1-3 h.
[0061] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and sample.
[0062] According to one aspect of the present invention, a fuel cell metal bipolar plate gradient composite coating proton exchange membrane fuel cell is provided, wherein the bipolar plate gradient composite coating proton exchange membrane fuel cell comprises the above-mentioned metal bipolar plate nano-array gradient composite coating.
[0063] The technical solution of the present invention will be further described below in conjunction with embodiments.
[0064] Example 1
[0065] A method for preparing a gradient composite coating on the surface of a bipolar plate:
[0066] (1) Cut 316L stainless steel sheets into 50×50 mm metal sheets by electric spark cutting, ultrasonically clean them with acetone, deionized water and anhydrous ethanol for 30 minutes in sequence, and then blow dry them with nitrogen.
[0067] (2) The cleaned 316L stainless steel sheet was clamped on the rotating table in the high-power impulse magnetron sputtering (HiPIMS) furnace, with a circular Ti target above the sample and the inter-electrode distance between the sample and the target maintained at 10 cm.
[0068] (3) Close the chamber, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10 -4 Pa, so that the furnace maintains a high vacuum state.
[0069] (4) Fill the furnace with high-purity Ar gas to keep the total pressure constant at 0.3 Pa during deposition, and heat the substrate to 100°C. After heating, turn on the substrate bias power supply to apply a negative bias of 600V, and sputter the substrate surface for 30 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0070] (5) Reduce the negative bias voltage of the substrate to 60 V, turn on the Ti target and increase the current linearly to 5 A within 1 min, maintain for 30 min, and obtain a metal gradient layer.
[0071] (6) Then, a layer of 3000 mesh stainless steel mesh was covered on the sample. The thickness of the stainless steel mesh was 2 mm, and the distance between the stainless steel mesh and the sample was kept at 0.5 cm. The target current and the total working pressure were kept constant, and high-purity C2H2 was linearly introduced within 1 min, with the flow ratio of Ar:C2H2 being 6:1. This was maintained for 3 h to obtain the display structure layer.
[0072] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and take samples.
[0073] This embodiment uses high-power pulsed magnetron sputtering HiPIMS technology to plasma clean 316L stainless steel to clean and activate its surface, which can etch impurity atoms and form a certain concentration of vacancies. On the basis of sputtering Ti transition layer (50nm) with HiPIMS technology, a 3000-mesh stainless steel mesh is covered on the substrate, and then a certain proportion of C2H2 is introduced into the chamber, and finally a nano-array structured metal carbide coating (200nm) with high bonding strength is obtained.
[0074] Figure 1 This is a schematic diagram of the preparation principle of the array gradient composite coating on the surface of the bipolar plate of this embodiment.
[0075] Figure 2 This is a comparison diagram of the surface morphology of the bipolar plate with an array gradient composite coating on the surface prepared in this embodiment and a 316L stainless steel sheet without a coating.
[0076] Figure 3 This is a comparison chart of contact angle values of the bipolar plate with an array gradient composite coating on its surface prepared in this embodiment and the surface of a 316L stainless steel sheet without a coating.
[0077] Figure 4 This is a comparison chart of the contact angle values of the array gradient composite coating on the surface of the bipolar plate of this embodiment.
[0078] Figure 5 This is a comparison chart of the corrosion current values of the array gradient composite coating on the surface of the bipolar plate of this embodiment.
[0079] Depend on Figures 1 to 5 It can be seen that the present application can prepare a nano-gradient composite coating with an array structure. High-energy HiPIMS sputtering can form a high concentration of vacancies on the substrate surface. Through process control, a Ti transition layer with a gradient distribution can be prepared, which helps to enhance the bonding performance of the composite coating. In addition, the special dot structure on the surface of the nano-array coating helps to increase the actual contact area with the carbon paper (GDL) and reduce the interfacial contact resistance (ICR); the rough structure on the coating surface is super-hydrophobic, which can hinder the adsorption of corrosive ions and enhance corrosion resistance.
[0080] Example 2
[0081] A method for preparing a gradient composite coating on the surface of a bipolar plate:
[0082] (1) A 316L stainless steel sheet was cut into metal sheets of 50 × 50 mm by electric spark cutting, and ultrasonically cleaned with acetone, deionized water, and anhydrous ethanol for 30 minutes in sequence, and then dried with nitrogen.
[0083] (2) The cleaned 316L stainless steel sheet was clamped on the rotating table in the high-power impulse magnetron sputtering (HiPIMS) furnace, with a circular Nb target above the sample, and the inter-electrode distance between the sample and the target was maintained at 10 cm.
[0084] (3) Close the cavity, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10-4Pa to maintain a high vacuum state in the furnace.
[0085] (4) Fill the furnace with high-purity Ar gas to keep the total pressure constant at 0.3 Pa during deposition, and heat the substrate to 100°C. After heating, turn on the substrate bias power supply to apply a negative bias of 600V, and sputter the substrate surface for 30 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0086] (5) Then, a layer of 3000 mesh Ti mesh was covered on the sample. The thickness of the Ti mesh was 2 mm, and the distance between the Ti mesh and the sample was kept at 0.5 cm. The substrate negative bias voltage was reduced to 60 V, and the Nb target current was turned on and increased linearly to 5 A within 1 min and maintained for 1 h. The thickness of the obtained metal gradient layer was 100 nm.
[0087] (6) The 3000-mesh Ti mesh was removed, the target current and the total working pressure were maintained unchanged, and high-purity N2 was linearly introduced within 1 min with an Ar:N2 flow ratio of 5:1. The flow was maintained for 2 h, and the thickness of the obtained display structure layer was 50 nm.
[0088] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and sample.
[0089] This embodiment uses high-power pulsed magnetron sputtering HiPIMS to sputter an array-structured Nb transition layer (100nm) on the surface of the substrate. During the stamping process, the array-structured Nb transition layer can provide a higher bonding strength for the composite coating, making the coating less prone to cracking and failure. At the same time, this embodiment can prepare a nano-metal carbon / nitride composite coating with high bonding strength by adding high-purity nitrogen during the sputtering process. During the stamping process, the array-structured Nb transition layer can provide a higher bonding strength for the composite coating, facilitating one-time molding that is not prone to adhesion, falling off and failure. In addition, the array-structured Nb transition layer helps to form a highly crystalline, highly chemically combined metal carbon / nitride nanocrystalline coating, and the coating surface has a high degree of integrity and density, which can improve electrical conductivity and corrosion resistance.
[0090] Example 3
[0091] A method for preparing a metal bipolar plate comprises the following steps:
[0092] (1) The metal substrate was mechanically cut into metal sheets of 50×50 mm in size, and ultrasonically cleaned with acetone, deionized water, and anhydrous ethanol for 30 minutes in sequence, and then dried with nitrogen.
[0093] (2) The cleaned metal substrate was placed on a rotating table in a high-power impulse magnetron sputtering (HiPIMS) furnace to ensure uniformity of coating preparation, and the distance between the target and the sample was kept at 20 cm.
[0094] (3) Cover the sample with a 5000 mesh metal mesh with a thickness of 5 mm and keep the distance between the metal mesh and the sample at 5 cm.
[0095] (4) Close the chamber, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10 -4 Pa, so that the furnace maintains a high vacuum state.
[0096] (5) The furnace is filled with high-purity Ar gas, the total pressure is kept constant at 2 Pa during deposition, and the substrate is heated to 200°C. After heating, the substrate bias power supply is turned on to apply a negative bias voltage of 600V, and the substrate surface is sputtered for 30 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0097] (6) Reduce the negative bias voltage of the substrate to 100 V, turn on the target current and increase it linearly to 1-5 A within 10 minutes, and maintain it for 30 minutes; maintain the target current and the total working pressure unchanged, and linearly introduce high-purity reaction gas within 10 minutes, with an Ar: reaction gas flow ratio of 1:1, and maintain it for 1 hour.
[0098] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and sample.
[0099] Example 4
[0100] A method for preparing a metal bipolar plate comprises the following steps:
[0101] (1) The metal substrate was mechanically cut into metal sheets of 50×50 mm in size, and ultrasonically cleaned with acetone, deionized water, and anhydrous ethanol for 30 minutes in sequence, and then dried with nitrogen.
[0102] (2) The cleaned metal substrate was placed on a rotating table in a high-power impulse magnetron sputtering (HiPIMS) furnace to ensure uniformity of coating preparation, and the distance between the target and the sample was kept at 5 cm.
[0103] (3) Cover the sample with a 1000 mesh metal mesh with a thickness of 0.1 mm and keep the distance between the metal mesh and the sample at 0.1 cm.
[0104] (4) Close the chamber, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10 -4 Pa, so that the furnace maintains a high vacuum state.
[0105] (5) Fill the furnace with high-purity Ar gas, keep the total pressure constant at 0.1-2 Pa during deposition, and heat the substrate to 50°C. After heating, turn on the substrate bias power supply to apply a negative bias of 400V, and sputter the substrate surface for 10 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0106] (6) Reduce the negative bias voltage of the substrate to 10 V, turn on the target current and increase it linearly to 1-5 A within 1-10 min, and maintain it for 10 min; maintain the target current and the total working pressure unchanged, and linearly introduce high-purity reaction gas within 1 min, with an Ar: reaction gas flow ratio of 10:1, and maintain it for 3 h.
[0107] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and sample.
[0108] Example 5
[0109] A method for preparing a metal bipolar plate comprises the following steps:
[0110] (1) The metal substrate was mechanically cut into metal sheets of 50×50 mm in size, and ultrasonically cleaned with acetone, deionized water, and anhydrous ethanol for 30 minutes in sequence, and then dried with nitrogen.
[0111] (2) The cleaned metal substrate was placed on a rotating table in a high-power impulse magnetron sputtering (HiPIMS) furnace to ensure uniformity of coating preparation, and the distance between the target and the sample was kept at 10 cm.
[0112] (3) Cover the sample with a 2000 mesh metal mesh with a thickness of 2 mm and keep the distance between the metal mesh and the sample at 2 cm.
[0113] (4) Close the chamber, turn on the plasma sputtering equipment and its matching cold water pump, and use a molecular pump to pump the gas pressure of the coating furnace to 6×10 -4 Pa, so that the furnace maintains a high vacuum state.
[0114] (5) Fill the furnace with high-purity Ar gas, keep the total pressure constant at 0.1-2 Pa during deposition, and heat the substrate to 100°C. After heating, turn on the substrate bias power supply to apply a negative bias of 500V, and sputter the substrate surface for 20 minutes; plasma sputtering can clean the substrate surface to remove impurity atoms and activate the surface to facilitate the adsorption of active atoms.
[0115] (6) Reduce the negative bias voltage of the substrate to 10 V, turn on the target current and increase it linearly to 1-5 A within 5 minutes, and maintain it for 10-30 minutes; maintain the target current and the total working pressure unchanged, and linearly introduce high-purity reaction gas within 5 minutes, with an Ar: reaction gas flow ratio of 5:1, and maintain it for 2 hours.
[0116] (7) After the plasma sputtering is completed, turn off the DC power supply, substrate bias, and gas source in sequence, cool the furnace to room temperature, and then vent and sample.
[0117] Experimental Example 1
[0118] In order to show that the metal bipolar plate gradient composite coating prepared in the present application has high conductivity and corrosion resistance, the metal bipolar plates prepared in Examples 1-5 of the present application are now subjected to performance tests, as follows:
[0119] 1. Potentiodynamic corrosion current test environment: 80℃, pH=3 (H2SO4), containing 0.1ppm F - , the scanning range is -0.5V~1.5V, and the scanning rate is 2mV / s.
[0120] 2. High potential accelerated durability test environment: Test conditions: 80°C, pH=3 (H2SO4), containing 2ppm F - , set the voltage to 1.6V (vs. SHE), test time 12h;
[0121] 3. Contact resistance test: According to the national standard GB / T 20042.6-2011, the contact resistance between the gradient composite coating of the metal bipolar plate and the Toray double-sided carbon paper is tested. The test pressure value is 0.1-2.0MPa (taking points 0.1, 0.2, 0.3...), and the test area is 25cm 2 .
[0122] The results are shown in Table 1 below:
[0123] Table 1
[0124]
[0125] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A gradient composite coating for metal bipolar plates of fuel cells, It is characterized in that The metal bipolar plate includes a substrate and a nano-array gradient composite coating deposited on the surface of the substrate; The nano-array gradient composite coating comprises an array structure layer, and the array structure layer is obtained by arranging a metal mesh above a substrate and then performing physical vapor deposition.
2. The bipolar plate gradient composite coating according to claim 1, It is characterized in that The nano-array gradient composite coating also includes a metal gradient layer; Preferably, the metal bipolar plate comprises a substrate, a metal gradient layer and an array structure layer in sequence; Preferably, the metal bipolar plate comprises a substrate, an array structure layer and a metal gradient layer in sequence.
3. The bipolar plate gradient composite coating according to claim 1, It is characterized in that The thickness of the nano-array gradient composite coating is 100-250 nm.
4. The bipolar plate gradient composite coating according to claim 1, It is characterized in that The substrate includes any one of 316L stainless steel, titanium steel or titanium plate.
5. The bipolar plate gradient composite coating according to claim 1, It is characterized in that The physical vapor deposition target includes at least one of a Ti target, a Nb target and a Cr target.
6. The bipolar plate gradient composite coating according to claim 1, It is characterized in that The metal mesh includes at least one of a stainless steel mesh, a titanium mesh and a copper mesh.
7. A method for preparing a gradient composite coating for a bipolar plate according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: The substrate is ion-etched to obtain an activated surface, and then subjected to physical vapor deposition to obtain a metal gradient layer; a metal mesh is then arranged on top of the metal gradient layer and subjected to physical vapor deposition to obtain a nano-array gradient composite coating; Alternatively, a metal mesh is arranged on the substrate and subjected to physical vapor deposition to obtain a metal transition layer having an array structure, and then physical vapor deposition is performed on the metal transition layer to obtain a nano-array gradient composite coating.
8. The method for preparing the gradient composite coating of a bipolar plate according to claim 7, It is characterized in that The physical vapor deposition is carried out under high-purity reaction gas; Preferably, the high-purity reaction gas includes Ar, C 2 H 2 and N 2 .
9. The method for preparing the gradient composite coating of a bipolar plate according to claim 7, It is characterized in that The preparation method further comprises the step of pretreating the substrate to be treated; Preferably, the pretreatment comprises: cutting the substrate to be treated into metal sheets of 50×50 mm in size, then ultrasonically cleaning with acetone, deionized water and anhydrous ethanol for 30 minutes in sequence, and then drying with nitrogen.
Citation Information
Cited By
Method for treating a structural component of an electrochemical cell and coated structural component
WO2026125633A3