Surface passivation microcavity, optical device and preparation method and application of surface passivation microcavity
By depositing an inert molecular layer on the surface of the whispering gallery microcavity, the problem of unstable optical frequency comb output caused by optical loss on the microcavity surface is solved, and long-term stable optical frequency comb output and low power threshold are achieved in an open air environment.
Patent Information
- Application Number
- CN202310355930.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
During the use and storage of the whispering gallery microcavity, the optical loss on the surface gradually increases, resulting in unstable optical frequency comb output and limiting its application prospects.
An inert molecular layer is used for surface modification to suppress the optical loss on the surface of the whispering gallery microcavity. A saturated aliphatic hydrocarbon or silane molecular layer is deposited through chemical vapor deposition to form a monomolecular layer to reduce light absorption and light scattering.
In an open air environment without the protection of dry nitrogen packaging, the long-term stable output of the whispering gallery microcavity optical frequency comb is achieved, the power threshold is kept low, and the fluctuation of optical parameters is less than 10%, extending the service life of the equipment.
Smart Images

Figure CN118783239A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of micro-nano devices, and in particular to a surface passivated microcavity, an optical device, and a preparation method and application thereof. Background Art
[0002] An optical frequency comb is a broadband coherent light source composed of a series of laser components with the same spacing and constant phase difference in the frequency domain. The optical frequency comb appears as equally spaced comb teeth in frequency, similar to a ruler, and as a light pulse in the time domain. Each comb ruler of the optical frequency comb is strictly equally spaced and has a constant phase difference. Through Fourier transform, the mode-locked comb rulers are coherently superimposed, and the ultra-short light pulses in the time domain are called solitons. The pulse period is the inverse of the repetition frequency, and the pulse width is the inverse of the spectrum span.
[0003] As a special optical resonant cavity, the whispering gallery microcavity constrains the light field on the annular boundary to cause continuous total reflection. When the optical path of the light beam propagating around the boundary of the geometric structure satisfies an integer multiple of the wavelength, an optical frequency resonance phenomenon will occur. Therefore, the whispering gallery microcavity can modulate the pump light of a wide spectrum, so that the pump light is self-coherently enhanced during the resonant transmission of the whispering gallery microcavity and produces an optical frequency comb output, wherein the comb tooth frequency of the optical frequency comb output by the whispering gallery microcavity is in the optical band, and its repetition frequency can range from the microwave band of 50MHz to the terahertz band of 10THz, thus establishing a link between light waves and microwaves and terahertz waves. Optical frequency combs have important application prospects in many fields such as coherent optical communications, ultrafast ranging, astronomical spectral analysis, optical atomic clocks, and ultra-low phase noise microwave generation.
[0004] However, the whispering gallery microcavity uses air as the device's coating layer. During use and storage, the optical loss on the microcavity surface will continue to increase over time, causing the power threshold of the microcavity optical frequency comb to increase rapidly, seriously affecting the generation and output stability of the optical frequency comb. In current applications, only dry nitrogen can be used to encapsulate and protect the whispering gallery microcavity, which can temporarily keep the optical frequency comb output of the whispering gallery microcavity stable for a period of time. However, even under the protection of dry nitrogen encapsulation, the optical loss on the whispering gallery microcavity surface will still slowly increase, ultimately resulting in the inability to generate an optical frequency comb. Therefore, the problem of optical loss on the whispering gallery microcavity surface is one of the key technical difficulties currently limiting the application of whispering gallery microcavity optical frequency comb technology.
[0005] Therefore, it is necessary to design a surface passivated microcavity, an optical device, and a preparation method and use thereof to solve the above problems. Summary of the invention
[0006] In view of the above shortcomings of the prior art, the present invention provides a surface-passivated microcavity, an optical device, and a preparation method and use thereof, which utilizes a surface-modified inert molecular layer to passivate the active surface of the whispering gallery microcavity, thereby effectively suppressing the increase of surface optical loss of the whispering gallery microcavity with storage, thereby solving the technical problem in the prior art that the whispering gallery microcavity cannot produce a stable optical frequency comb output due to surface optical loss.
[0007] To achieve the above-mentioned object and other related objects, the present invention provides a surface passivation microcavity, which comprises: a whispering gallery microcavity and an inert molecular layer.
[0008] Wherein, an inert molecular layer is attached to the surface of the whispering gallery microcavity, and the inert molecular layer suppresses optical loss on the surface of the whispering gallery microcavity, and the optical loss at least includes light absorption and light scattering.
[0009] In one example of the present invention, the inert molecular layer is a monomolecular layer.
[0010] In an example of the present invention, the material of the inert molecular layer includes saturated aliphatic hydrocarbon molecules or silane molecules.
[0011] In one example of the present invention, the saturated aliphatic hydrocarbon molecules include saturated aliphatic hydrocarbon molecules of different chain lengths and fluorinated saturated aliphatic hydrocarbon molecules.
[0012] In an example of the present invention, the structure of the whispering gallery microcavity includes a spherical type, a disk-on-chip type, a wedge-shaped cavity on a chip, an annular core type on a chip, a microbottle type or a microbubble type.
[0013] In an example of the present invention, the material of the whispering gallery microcavity is organic siloxane and / or inorganic silicon oxide.
[0014] Another aspect of the present invention provides an optical device, comprising a pump light waveguide, a signal light waveguide and a surface passivated microcavity as described in any one of the above examples; wherein the pump light waveguide and the signal light waveguide are coupled to the surface passivated microcavity.
[0015] Another aspect of the present invention provides a use of the surface passivated microcavity described in any of the above examples in an optical device, wherein the optical device generates a stable laser output under the same pump light excitation in an open air environment, and can be further applied to highly integrated optical devices, such as high-sensitivity detectors, low-threshold micro-lasers on chips, amplifiers, filters and modulators in optical communication networks, etc. The stable laser output is an output laser whose optical parameters fluctuate less than 10% as the storage and use time of the optical device increases, and the optical parameters include the power threshold, mode number and mode frequency of the output laser.
[0016] In an example of the present invention, the laser output may be an optical frequency comb output.
[0017] On the other hand, the present invention also provides a method for preparing a surface-passivated microcavity, the preparation method comprising the following steps: preparing a whispering gallery microcavity; depositing an inert molecular layer on the surface of the whispering gallery microcavity by chemical vapor deposition; and cleaning and vacuum drying the whispering gallery microcavity after the reaction to obtain a surface-passivated whispering gallery microcavity.
[0018] The surface passivated microcavity, optical device, preparation method and use thereof of the present invention modify an inert molecular layer on the surface of the whispering gallery microcavity, and utilize the inert molecular layer to passivate the active surface of the whispering gallery microcavity, thereby effectively suppressing the significant increase of optical loss on the surface of the whispering gallery microcavity during storage and use, and stabilizing the sensitive light and heat balance inside the whispering gallery microcavity during long-term storage, so that the whispering gallery microcavity can achieve stable locking and output of the optical frequency comb for a long time in an open air environment without dry nitrogen packaging protection.
[0019] In summary, the surface passivated microcavity can effectively suppress the surface optical loss of the microcavity during long-term use or storage in an open air environment without dry nitrogen packaging protection, thereby achieving long-term stable output of the low-power threshold optical frequency comb. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 FIG. 1 is a schematic diagram of the structure of a surface passivated microcavity in one embodiment of the present invention.
[0022] Figure 2 The optical frequency comb spectra of the whispering gallery microcavity in one embodiment of the present invention are compared when the surface is modified with an inert molecular layer and when it is excited by a 1550nm pump light. (a) is the optical frequency comb spectrum of the microcavity without surface modification and excited by a 1550nm pump light during long-term storage in an air environment; (b) is the optical frequency comb spectrum of the microcavity with surface modification and excited by a 1550nm pump light during long-term storage in an air environment.
[0023] Figure 3 This is a test chart of the optical frequency comb output power of a surface-passivated microcavity excited by 1550nm pump light in one embodiment of the present invention.
[0024] Figure 4 This is a graph showing the change in excitation power threshold of the optical frequency comb output under 1550nm pump light during long-term storage of a whispering gallery microcavity with surface modification in one embodiment of the present invention.
[0025] Component number description
[0026] 100. Whispering gallery microcavity; 200. Inert molecular layer. DETAILED DESCRIPTION
[0027] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.
[0028] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.
[0029] The inventors have found through research that a whispering gallery microcavity with an ultra-high quality factor can produce an optical frequency comb output with a low power threshold when it is just prepared. However, the surface of the whispering gallery microcavity is active. During the storage and use of the whispering gallery microcavity, the optical loss of the active surface gradually increases, causing the performance of the optical frequency comb output of the whispering gallery microcavity to deteriorate until it is completely unable to produce an optical frequency comb output. At present, the existing method usually requires the whispering gallery microcavity to be precisely encapsulated in a dry inert gas in order to stabilize the optical frequency comb output of the whispering gallery microcavity. However, even under the protection of strict dry inert gas encapsulation, the optical loss on the surface of the whispering gallery microcavity will still slowly increase during the storage and use process, and destroy the light and heat balance in the whispering gallery microcavity, resulting in the whispering gallery microcavity being unable to guide the resonant light in the cavity to lock the optical frequency comb mode, and thus being unable to produce an optical frequency comb output.
[0030] Therefore, the present invention provides a surface passivated microcavity, which utilizes an inert molecular layer to passivate the surface of the whispering gallery microcavity, so as to effectively suppress the significant increase of optical loss on the surface of the whispering gallery microcavity during storage and use, stabilize the sensitive light and heat balance inside the whispering gallery microcavity during long-term storage, and enable the whispering gallery microcavity to achieve stable locking and output of the optical frequency comb frequency mode for a long time in an open air environment without dry nitrogen packaging protection.
[0031] See also Figure 1 The surface passivated microcavity includes a whispering gallery microcavity 100 and an inert molecular layer 200. The surface of the whispering gallery microcavity 100 is modified with the inert molecular layer 200, which is densely attached to the surface of the whispering gallery microcavity 100 and completely covers the whispering gallery microcavity 100.
[0032] like Figure 1 As shown, the inert molecular layer 200 can completely replace the active surface of the whispering gallery microcavity 100. The introduction of the inert molecular layer 200 on the surface of the whispering gallery microcavity 100 will not change the effective refractive index and dispersion of the cavity itself, and can also isolate the adsorption of substances on the surface of the whispering gallery microcavity 100 to the external air environment during the use or storage of the whispering gallery microcavity 100, stabilize the sensitive light and heat balance inside the whispering gallery microcavity 100, and avoid the light absorption and light scattering loss caused by the uneven surface when the resonant light is resonantly transmitted along the surface of the whispering gallery microcavity 100, and the mode frequency migration caused by the sudden change of the resonant light optical path, thereby playing a role in suppressing the surface optical loss during the use and storage of the whispering gallery microcavity 100, and realizing the stable output of the optical frequency conversion laser by the whispering gallery microcavity 100. Among them, the optical frequency conversion output that the whispering gallery microcavity 100 can generate under the excitation of pump light includes at least one frequency conversion of Kerr optical frequency sparseness, soliton optical frequency sparseness, stimulated Raman scattering, and stimulated Brillouin scattering.
[0033] like Figure 2 and Figure 4 As shown, the surface passivated microcavity can achieve stable laser output due to the introduction of the inert molecular layer. The stable laser output is a laser output with constant optical parameters generated by the surface passivated microcavity under the same pump light excitation, wherein the constant optical parameters include constant power and constant mode. The constant power is manifested in that the power threshold of the laser output generated by the surface passivated microcavity under the same pump light excitation does not change with time, and the constant mode is manifested in that the mode frequency and mode number of the laser output generated by the surface passivated microcavity under the same pump light excitation do not change with time.
[0034] In some embodiments, the surface passivated microcavity has a stable optical frequency comb output, and the stable optical frequency comb output means that the surface passivated microcavity generates an optical frequency comb output whose mode and power do not change with storage and use time under the same pump light excitation. Specifically, it can be manifested that the optical parameters of the optical frequency comb output by the surface passivated microcavity do not change with storage and use time, wherein the optical parameters include the power threshold, mode frequency and mode number of the optical frequency comb generated by the surface passivated microcavity, and the constancy of the mode frequency and mode number is manifested in that the spectrum width of the optical frequency comb, the number of comb tooth peaks and the frequency of each comb tooth peak do not change with time. For example, Figure 2 and 4 As shown, when the surface passivated microcavity is stored or used in an open air environment without dry nitrogen packaging protection, the power threshold of the optical frequency comb generated by the surface passivated microcavity remains constant, and the comb tooth frequency, number of comb teeth and spectrum width of the surface passivated microcavity optical frequency comb output also remain constant and do not increase with the extension of storage or use time.
[0035] It should be noted that, in the present invention, the cavity material of the whispering gallery microcavity is not limited, and the cavity material of the whispering gallery microcavity can be any one of silicon, silicon nitride, organosiloxane, inorganic silicon oxide, chalcogenide glass and lithium niobate. In some embodiments, the cavity material of the whispering gallery microcavity can be an inorganic silicon oxide, and further, the cavity material of the whispering gallery microcavity can be silicon dioxide, for example, the whispering gallery microcavity can be silicon dioxide, doped silicon dioxide or quartz.
[0036] Among them, the whispering gallery microcavity made of silica has the highest quality factor, can achieve ultra-low threshold optical frequency comb generation, significantly reduce the pump power requirement of optical frequency comb devices, and is one of the most promising micro optical frequency comb devices. However, due to the active surface of the silica whispering gallery microcavity, the optical loss of the microcavity surface in the air environment will increase over time, causing the power threshold of the microcavity optical frequency comb to increase rapidly, and the output frequency of the optical frequency comb to be distorted, which seriously affects the generation and output stability of the optical frequency comb.
[0037] In some embodiments, the material of the inert molecular layer includes saturated aliphatic hydrocarbon molecules or silane molecules. Among them, the saturated aliphatic hydrocarbon molecules include saturated aliphatic hydrocarbon molecules of different chain lengths and fluorinated saturated aliphatic hydrocarbon molecules. In the above embodiments, the saturated aliphatic hydrocarbon molecules can be attached to the surface of the silica whispering gallery microcavity through hydrophobic silane bonds, thereby replacing the active surface of the silica whispering gallery microcavity with an inert molecular layer, avoiding the increase of optical loss on the surface of the silica whispering gallery microcavity over time, so as to achieve a stable optical frequency comb output.
[0038] In some embodiments, the inert molecular layer is modified on the surface of the whispering gallery microcavity in the form of a monomolecular layer. The monomolecular inert molecular layer does not introduce additional optical loss when modifying the surface of the whispering gallery microcavity, and can effectively ensure the high quality factor of the whispering gallery microcavity itself. Among them, if the inert molecular layer is modified on the surface of the whispering gallery microcavity in the form of multiple layers, the introduction of multiple layers of inert molecular layers is likely to produce absorption and scattering effects on the resonant light in the whispering gallery microcavity, thereby reducing the quality factor of the whispering gallery microcavity.
[0039] In addition, in the present invention, the structure of the whispering gallery microcavity is not limited. For example, the structure of the whispering gallery microcavity can be spherical, on-chip disk, on-chip wedge-shaped cavity, on-chip ring core, microbottle or microbubble. In some embodiments, the whispering gallery microcavity can be a spherical microcavity.
[0040] The present invention also provides a method for preparing a surface passivated microcavity, the method comprising the following steps:
[0041] S1. Preparation of whispering gallery microcavity;
[0042] S2, depositing an inert molecular layer on the surface of the whispering gallery microcavity by chemical vapor deposition;
[0043] S3, cleaning and vacuum drying the whispering gallery microcavity after the reaction to obtain a surface passivated whispering gallery microcavity.
[0044] In step S1, the whispering gallery microcavity can be prepared by conventional preparation methods in the art. For example, taking a spherical microcavity as an example, a microspherical whispering gallery microcavity is fired by melting the fiber cone using a carbon dioxide laser (the laser light source wavelength is 1550nm, and lasers of other bands can also be used). Among them, it should be noted during firing that the spherical microcavity is kept sufficiently vertical to the fiber handle so as to find the equatorial plane of the spherical microcavity during subsequent coupling of the optical waveguide. Specifically, there are two key points: 1) The connection between the fiber cone and the spherical microcavity should be as thin as possible. If the connection is too thick, the spherical microcavity will tilt toward the laser side. For example, in this example, the connection between the spherical microcavity and the fiber cone is about 4-5μm; 2) Appropriate power should be used for melting. If the laser output power is too high, the prepared spherical microcavity will be too small. If the laser output power is too high, the spherical microcavity will tilt in the opposite direction of the laser injection.
[0045] In step S2, the whispering gallery microcavity is first placed in an oxygen cleaning machine so that the whispering gallery microcavity is cleaned under oxygen plasma to ensure that a dense layer of hydroxyl groups is suspended on the surface of the whispering gallery microcavity; then an inert molecular material is deposited on the surface of the whispering gallery microcavity using chemical vapor deposition, and the inert molecular material reacts with the hydroxyl groups to convert the hydroxyl groups on the surface of the whispering gallery microcavity into an inert molecular layer.
[0046] The inert molecular material in step S2 can be aliphatic hydrocarbon molecules or silane molecules, and the saturated aliphatic hydrocarbon molecules include saturated aliphatic hydrocarbon molecules with different chain lengths and fluorinated saturated aliphatic hydrocarbon molecules.
[0047] In step S3, the surface of the whispering gallery microcavity is cleaned with a solvent that deposits inert molecules, and after cleaning, it is placed in a vacuum drying oven for vacuum drying for several minutes and then taken out to obtain a surface passivated microcavity.
[0048] The present invention also provides an optical device, comprising a pump light waveguide, a signal light waveguide and the surface passivated microcavity described in any one of the above embodiments, wherein the pump light waveguide and the signal light waveguide are coupled to the surface passivated microcavity as a pump light input end and a signal light output end, respectively, and the coupling ends of the pump light waveguide and the signal light waveguide to the surface passivated microcavity are optical fiber cones.
[0049] The preparation process of the optical device is as follows: the fiber cones of the pump light waveguide and the signal light waveguide are melt-stretched using a hydrogen flame gun and a stepper motor. The side with a smaller curvature of the fiber cones of the pump light waveguide and the signal light waveguide is used to couple the surface passivated microcavity, so as to couple the surface passivated microcavity. The fiber cones of the pump light waveguide and the signal light waveguide are coupled to the microcavity through a precision translation stage. The preparation method of the surface passivated microcavity is as described above.
[0050] The present invention also provides the use of the surface passivated microcavity described in any of the above embodiments in an optical device, wherein the optical device generates a stable laser output under the same pump light excitation in an open air environment, and can be further applied to highly integrated optical devices, such as high-sensitivity detectors, low-threshold micro-lasers on chips, amplifiers, filters and modulators in optical communication networks, etc. Among them, the stable laser output is an output laser whose optical parameters fluctuate by less than 10% as the placement and use time of the optical device increases, wherein the optical parameters include the power threshold, mode number and mode frequency of the output laser generated by the optical device. Specifically, the power and mode of the laser output generated by the optical device under the same pump light excitation will not change with the increase of storage and use time.
[0051] In some embodiments, the use includes the application of an optical device generating a stable optical frequency comb output under pump light excitation, wherein the stable optical frequency comb output is an optical frequency comb output whose mode and power do not change with storage and use time under the same pump light excitation. Specifically, it can be manifested that the optical parameters of the optical frequency comb output by the optical device do not change with storage and use time, wherein the optical parameters include the power threshold, mode frequency and mode number of the optical frequency comb generated by the optical device, and the constant mode frequency and mode number of the optical frequency comb are manifested in that the spectrum width of the optical frequency comb, the number of comb tooth peaks and the frequency of each comb tooth peak do not change with time.
[0052] The technical scheme of the present invention is described in detail below through specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available products or can be prepared by conventional methods in the art.
[0053] Example 1
[0054] Example 1 A surface passivated microcavity with a surface modified with an inert molecular layer is prepared. The preparation process is as follows:
[0055] S1. Use a carbon dioxide laser with an output wavelength of 1550nm to melt the fiber cone to burn a microspherical whispering gallery microcavity with a diameter of 120μm;
[0056] S2, treating the whispering gallery microcavity with oxygen plasma so that the surface of the whispering gallery microcavity has a dense monolayer of hydroxyl groups, and then depositing fluorinated saturated aliphatic hydrocarbon molecules on the surface of the whispering gallery microcavity by chemical vapor deposition, so that the monolayer of hydroxyl groups on the surface of the whispering gallery microcavity is converted into fluorinated saturated aliphatic hydrocarbon molecules;
[0057] S3, cooling, cleaning and vacuum drying the whispering gallery microcavity after the reaction to obtain a surface passivated whispering gallery microcavity.
[0058] Comparative Example 1
[0059] Comparative Example 1: A whispering gallery microcavity without surface modification was prepared. The preparation process is as follows:
[0060] A carbon dioxide laser was used to melt the fiber taper to burn a microspherical whispering gallery microcavity with a diameter of 120 μm.
[0061] The following tests are conducted to compare the surface passivated microcavity of Example 1 and the unmodified whispering gallery microcavity of Comparative Example 1. The whispering gallery microcavities of Example 1 and Comparative Example 1 are stored in an open air environment. Figure 2 In the test optical path shown, a pump light with a wavelength of 1550nm is used to test the optical frequency comb output of the surface passivated microcavity and the whispering gallery microcavity without surface modification, so as to verify the contribution of the surface-modified inert molecular layer to the stable output of the optical frequency comb of the surface passivated microcavity.
[0062] The test results and conclusions are as follows:
[0063] like Figure 2As shown in the figure, both the newly prepared whispering gallery microcavity without surface modification and the surface passivated microcavity can generate optical frequency comb output under the excitation of 1550nm pump light of about 1.5mW. However, the surface optical loss of the whispering gallery microcavity without surface modification gradually increases in an open air environment, causing the optical frequency comb that the whispering gallery microcavity can output to attenuate until it disappears completely. Figure 2 As shown in (a), after being placed in an open air environment with non-dry nitrogen packaging for 7 days, the whispering gallery microcavity without surface modification can hardly produce optical frequency comb output under the same pump light excitation, and only individual parametric frequency signals can be observed; and after being placed in an open air environment with non-dry nitrogen packaging for 14 days, the whispering gallery microcavity without surface modification can completely fail to produce parametric frequency and cannot generate optical frequency comb output. On the contrary, the surface-modified inert molecular layer can effectively suppress the increase of optical loss on the surface of the whispering gallery microcavity, and achieve long-term stable output of the microcavity optical frequency comb, as shown in the figure. Figure 2 As shown in (b), the surface-passivated microcavity can generate stable optical frequency comb output under the same pump light excitation after being placed in an open air environment for 42 days and 100 days.
[0064] In addition, by comparing the optical frequency combs produced by the unmodified whispering gallery microcavity and the surface passivated microcavity when they were just prepared, it can be found that the optical frequency combs produced by the unmodified whispering gallery microcavity and the surface passivated microcavity under the same pump light excitation have very similar comb tooth peak frequency spacing and spectrum width, which indicates that the surface-modified inert molecular layer has no obvious effect on the effective refractive index and dispersion of the whispering gallery microcavity.
[0065] like Figure 3 and Figure 4 As shown in the figure, after being stored in an open air environment for a period of time, the optical frequency comb generated by the surface-passivated microcavity still has an ultra-low power threshold, which has been stable at around 120 microwatts. However, for the unmodified whispering gallery microcavity, due to the increase in surface absorption optical loss, the power threshold of the optical frequency comb generated by the unmodified whispering gallery microcavity also increases to around 89 milliwatts.
[0066] Specific as Figure 4 As shown in the figure, the surface passivated microcavity still has excellent stability even when placed in an open air environment protected by non-dry nitrogen packaging. The inert molecular layer modified on the surface of the surface passivated microcavity significantly inhibits the increase of optical loss on the cavity surface. During the test period of more than 300 days, the quality factor of the surface passivated microcavity remained unchanged and always maintained at 2.8×10 8 The power threshold of the optical frequency comb that can be produced by the surface passivated microcavity also remains unchanged, always maintained at around 120 microwatts.
[0067] In summary, this surface passivated microcavity can achieve long-term stable locking and output of the optical frequency comb in an air environment without dry nitrogen packaging protection.
[0068] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A surface passivated microcavity, characterized in that: include: Whispering gallery microcavity; An inert molecular layer is attached to the surface of the whispering gallery microcavity, and the inert molecular layer suppresses optical loss on the surface of the whispering gallery microcavity, wherein the optical loss at least includes light absorption and light scattering.
2. The surface passivated microcavity according to claim 1, characterized in that: The inert molecular layer is a monomolecular layer.
3. The surface passivated microcavity according to claim 1, characterized in that: The material of the inert molecular layer includes saturated aliphatic hydrocarbon molecules or silane molecules.
4. The surface passivated microcavity according to claim 3, characterized in that: The saturated aliphatic hydrocarbon molecules include saturated aliphatic hydrocarbon molecules of different chain lengths and fluorinated saturated aliphatic hydrocarbon molecules.
5. The surface passivated microcavity according to claim 1, characterized in that: The structures of the whispering gallery microcavity include spherical type, on-chip disk type, on-chip wedge-shaped cavity, on-chip ring core type, micro-bottle type or micro-bubble type.
6. The surface passivated microcavity according to claim 1, characterized in that: The material of the whispering gallery microcavity is organic siloxane and / or inorganic silicon-oxygen compound.
7. An optical device, characterized in that: include: A pump light waveguide, a signal light waveguide and a surface passivated microcavity according to any one of claims 1 to 6, wherein the pump light waveguide and the signal light waveguide are coupled to the organic hybrid microcavity.
8. Use of the surface passivated microcavity according to claims 1 to 6 in an optical device, characterized in that: The optical device generates stable laser output under pump light excitation, and the stable laser output is an output laser whose fluctuation amplitude of optical parameters over time is less than 10%, wherein the optical parameters include power threshold, mode number and mode frequency of the output laser.
9. The use according to claim 8, characterized in that The laser output is an optical frequency comb output.
10. A method for preparing a surface passivated microcavity, characterized in that: Preparation of whispering gallery microcavities; Depositing an inert molecular layer on the surface of the whispering gallery microcavity by chemical vapor deposition; The whispering gallery microcavity after the reaction is cleaned and vacuum dried to obtain a whispering gallery microcavity with a passivated surface.
Citation Information
Cited By
All-optical tuning controllable optical comb generation system and method based on functionalized micro-bottle cavity
CN119439536A