Process for preparing recovered bis (2-hydroxyethyl) terephthalate by multi-step depolymerization
Through multi-stage depolymerization and separation steps, the problems of purity and color quality of bis(2-hydroxyethyl)terephthalate in waste polyester are solved, achieving high purity and high quality recycling, suitable for polymers of efficient production.
Patent Information
- Application Number
- CN202380023514.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-25
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to ensure the high purity and high quality of bis(2-hydroxyethyl)terephthalate in the depolymerization process of waste polyester using existing technology, and it is difficult to effectively remove diethylene glycol and its derived impurities, which affects the polymer. physical properties and color quality.
Using multi-stage depolymerization and separation steps, including first and second glycolysis reactions, ion exchange and distillation, depolymerization is performed at 180°C to 200°C and 150°C to 170°C respectively, followed by removal of impurities through ion exchange resin Unreacted diol is removed at 150°C or lower, ultimately improving purity through distillation and adsorption-crystallization steps.
Significantly improves the purity and color quality of bis(2-hydroxyethyl)terephthalate, reduces the formation of diethylene glycol and its derived impurities, ensures excellent physical properties and color of the polymer, and is suitable for high-efficiency liquids Phase chromatography analysis.
Smart Images

Figure CN118786115A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing high-purity and high-quality recycled bis(2-hydroxyethyl)terephthalate (BHET) from waste polyester. Background Art
[0002] Polyester is one of the commonly used polymers in modern life. With its excellent mechanical strength, heat resistance, transparency and gas barrier properties, it is widely used as a material for beverage filling containers, packaging films, audio and video films, etc. In addition, polyester is widely produced worldwide as an industrial material, such as medical fibers and tire cords. In particular, polyester sheets or plates have good transparency and excellent mechanical strength, so they are widely used as raw materials for boxes, boxes, partitions, shelves, panels, packaging materials, building materials, interior and exterior materials, etc.
[0003] As a result, the amount of plastic waste such as polyester generated worldwide each year has reached an uncontrollable level. Recently, countries around the world are formulating regulations and plans for the recycling of waste plastic resources, including waste polyester. Although physical or chemical methods are used as methods for recycling waste polyester, physical recycling methods cannot guarantee purity and are not widely used.
[0004] In the chemical recycling method, the ester bonds of the waste polyester are broken to depolymerize it. Reactions such as glycolysis, hydrolysis, methanolysis and aminolysis are used. Glycolysis is the decomposition of the waste polyester by adding a glycol, such as ethylene glycol or diethylene glycol, at high temperature. A reaction product mainly containing bis(2-hydroxyethyl)terephthalate (BHET) is obtained.
[0005] Bis(2-hydroxyethyl)terephthalate can be used as a raw material for preparing unsaturated polyester or ester polyols after crystallization or purification.
[0006] [Prior art literature]
[0007] (Patent Document 1) Korean Patent No. 1386683
[0008] (Patent Document 2) U.S. Patent No. 7211193
[0009] (Non-patent document 1) Park, SH, Kim, SH, Poly(ethyleneterephthalate)recycling for high value added textiles, Fashion and Textiles 1, 1 (2014). Summary of the invention
[0010] Technical issues
[0011] Generally, the depolymerization reaction product of the waste polyester resin contains a large amount of oligomers such as dimers and trimers in addition to bis(2-hydroxyethyl)terephthalate (BHET). Since diethylene glycol (DEG) is formed at a high depolymerization temperature, side reaction products derived from diethylene glycol are inevitably formed.
[0012] For example, diethylene glycol ester (DEG ester) causes a decrease in physical properties when polymerizing recycled polyester resins, and to a greater extent in the case of polyester copolymers. In addition, it darkens and yellows the color of the polymerized raw material; therefore, its use is inevitably limited.
[0013] As a result of studies conducted by the present inventors to solve this problem, it has been found that high-purity BHET can be prepared by conducting a depolymerization reaction in multiple stages while significantly lowering the temperature of the latter stage, thereby reducing the formation of diethylene glycol and its derived impurities.
[0014] Furthermore, the present inventors were able to prepare BHET with enhanced color quality by further performing ion exchange and distilling unreacted diols after the depolymerization reaction, thereby reducing the formation of oligomers and removing chromophores.
[0015] Therefore, an object of the present invention is to provide a method for preparing high-purity and high-quality recycled bis(2-hydroxyethyl)terephthalate (BHET) using waste polyester through a multi-stage depolymerization reaction and separation and purification steps.
[0016] Solution to the problem
[0017] The present invention provides a method for preparing recycled bis(2-hydroxyethyl)terephthalate, which comprises (1) depolymerizing waste polyester by a first glycolysis reaction at a temperature of 180° C. to 200° C. to obtain a first reactant; (2) depolymerizing the first reactant by a second glycolysis reaction at a temperature of 150° C. to 170° C. to obtain a second reactant; (3) performing ion exchange on the second reactant by an ion exchange resin to obtain a third reactant; (4) removing unreacted diol from the third reactant by distillation at a temperature of 150° C. or lower to obtain a fourth reactant; and (5) distilling the fourth reactant to obtain crude bis(2-hydroxyethyl)terephthalate.
[0018] Furthermore, the present invention provides recovered bis(2-hydroxyethyl)terephthalate prepared by the above method, wherein the peak area fraction of bis(2-hydroxyethyl)terephthalate is 96% or more and the peak area fraction of diethylene glycol ester compounds is less than 2% in total when measured by high performance liquid chromatography (HPLC).
[0019] Advantageous Effects of the Invention
[0020] According to the method of the present invention, high-purity bis(2-hydroxyethyl)terephthalate (BHET) can be prepared by performing a depolymerization reaction in multiple stages while significantly reducing the temperature of the latter stage, thereby reducing the formation of diethylene glycol and its derived impurities. In addition, according to the method of the present invention, by further performing ion exchange and distilling unreacted diol after the depolymerization reaction, thereby reducing the formation of oligomers and removing chromophores, bis(2-hydroxyethyl)terephthalate (BHET) with enhanced color quality can be prepared.
[0021] Therefore, the present invention can not only depolymerize waste polyester to recover resources, but also use the recycled bis(2-hydroxyethyl)terephthalate produced according to the present invention as a raw material to produce polyester resins and products of excellent quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A method for preparing recycled bis(2-hydroxyethyl)terephthalate according to one embodiment is shown. DETAILED DESCRIPTION
[0023] Best Mode for Carrying Out the Invention
[0024] Hereinafter, various embodiments and examples will be described in detail with reference to the accompanying drawings.
[0025] In the present specification, the terms relating to the respective components are used to distinguish them from each other, and are not intended to limit the scope of the embodiments. In addition, in the present specification, unless otherwise specified in the context, singular expressions are also interpreted as covering the plural.
[0026] In this specification, the terms first, second, etc. are used to describe various components. However, these components should not be limited by these terms. These terms are only used to distinguish one element from another element.
[0027] In this specification, the term "comprising" is intended to specify specific features, regions, steps, methods, elements and / or components. Unless otherwise expressly stated, the existence or addition of any other features, regions, steps, methods, elements and / or components is not excluded.
[0028] According to the method for preparing recovered bis(2-hydroxyethyl)terephthalate of the present invention, the method comprises: (1) depolymerizing waste polyester by a first glycolysis reaction at a temperature of 180°C to 200°C to obtain a first reactant; (2) depolymerizing the first reactant by a second glycolysis reaction at a temperature of 150°C to 170°C to obtain a second reactant; (3) ion-exchanging the second reactant by an ion exchange resin to obtain a third reactant; (4) removing unreacted diol from the third reactant by distillation at a temperature of 150°C or lower to obtain a fourth reactant; and (5) distilling the fourth reactant to obtain crude bis(2-hydroxyethyl)terephthalate.
[0029] Prior to step (1), a step of crushing the waste polyester to a certain level or below may be further performed. Furthermore, a step of cooling the second reactant obtained in step (2) to a certain temperature or lower may be further performed. Furthermore, prior to step (3), a step of removing insoluble foreign matter from the second reactant by filtration may be further performed. Furthermore, after the distillation of step (5), a step of adsorption-crystallization of crude bis(2-hydroxyethyl)terephthalate may be further performed.
[0030] Figure 1 A method for preparing recycled bis(2-hydroxyethyl)terephthalate according to one embodiment is shown. Figure 1 , firstly, the waste polyester is crushed to a size of 4 mm or less to be prepared (S100), ethylene glycol is added thereto, and then a first glycolysis reaction is carried out at a temperature of 180°C to 200°C for about 2 hours in the presence of a zinc acetate catalyst (S210), and ethylene glycol is further added, and then a second glycolysis reaction is carried out at a temperature of 150°C to 170°C for about 2 hours (S220). Thereafter, it is cooled to 120°C or less using reduced pressure flash evaporation (S300), a small amount of filter aid is added thereto, and then it is filtered to separate insoluble foreign matter by solid-liquid separation (S400), and it is passed through a column filled with an ion exchange resin to perform ion exchange (S500). Then, unreacted diol is recovered at a temperature of 100° C. to 130° C. (S600), purified by thin film distillation at 190° C. to 250° C. (S700), and finally, an adsorption-crystallization step (S800) is performed to obtain high-purity and high-quality bis(2-hydroxyethyl)terephthalate.
[0031] Hereinafter, each step will be described in detail.
[0032] Preparation of waste polyester
[0033] The waste polyester used as a raw material in the present invention may be obtained from polyester material products discarded after use.
[0034] For example, waste polyester can be obtained from products such as beverage bottles, fabrics, films, cases, boxes, partitions, shelves, protective panels, packaging materials, building materials, and interior and exterior materials made of various polyester materials that are discarded by consumers after use.
[0035] The waste polyester material may be pre-treated before being subjected to the depolymerization step.
[0036] First, once other plastics, metals and foreign matter mixed in with the waste polyester material are removed, it will be cleaned and screened according to detailed characteristics such as color if necessary.
[0037] The waste polyester material thus screened is placed in a pulverizer and crushed into small pieces. The waste polyester flakes thus obtained can be screened to a desired particle size or smaller using a screen. The size of the screen can be, for example, 4 mm or smaller, 3 mm or smaller, or 2 mm or smaller.
[0038] The sieved flakes may be washed, hot air dried or similarly treated, and then proceed to a deagglomeration step.
[0039] Meanwhile, the waste polyester subjected to the glycolysis reaction can have a controlled particle size. For example, the waste polyester can be pulverized into a flake shape through the pretreatment step as described above.
[0040] Specifically, the particle size of the waste polyester may be 4 mm or less, 3 mm or less, 2 mm or less, or 1 mm or less. Within the above particle size range, the glycolysis reaction can be carried out under relatively low temperature conditions. For example, the temperature conditions of the first glycolysis reaction can be adjusted to 195°C or less, 190°C or less, 185°C or less, or 180°C, and the temperature conditions of the subsequent second glycolysis reaction can be adjusted to 160°C or less or 150°C or less. In addition, within the above particle size range, the glycolysis reaction can be carried out in a relatively short time. For example, starting from the time point when the appropriate temperature is reached, the time period of the first and second glycolysis reactions can be 3 hours or less, 2 hours or less, or 1 hour or less.
[0041] In addition, the waste polyester may have a fine structure similar to a fiber. For example, the waste polyester may be a waste fiber or a fiber material such as a waste banner.
[0042] As a specific example, the waste polyester may have a granular or fibrous form with a particle size of 4 mm or less.
[0043] The fiber may include at least one of a monofilament yarn and a multifilament yarn. The diameter of the monofilament yarn may be, for example, 0.05 denier to 100 deniers and may correspond to approximately 0.001 mm to 0.1 mm. Specifically, the monofilament yarn may have a diameter of 0.05 denier to 7 deniers or 7 deniers to 100 deniers. The diameter of the multifilament yarn may be, for example, 1 denier to 10,000 deniers and may correspond to approximately 0.01 mm to 1 mm. Specifically, the multifilament yarn may have a diameter of 0.01 denier to 0.2 deniers or 0.2 deniers to 1 deniers.
[0044] If the particle size or diameter of the waste polyester is adjusted within a specific range for depolymerization, the solvation can be accelerated even under relatively low temperature and short reaction time conditions.
[0045] Specifically, according to the present invention, a two-stage glycolysis reaction (i.e., a first glycolysis reaction and a second glycolysis reaction) is performed. If the solvation is accelerated in the first glycolysis reaction, the transesterification reaction of the waste polyester can be performed under the conditions of a lower temperature and a short reaction time in the second glycolysis reaction. Therefore, the concentration of diethylene glycol (DEG) naturally formed at a normal glycolysis reaction temperature can be significantly reduced, and the content of diethylene glycol ester compounds (DEG esters) in the recovered bis(2-hydroxyethyl) terephthalate finally prepared can be significantly reduced.
[0046] The diethylene glycol ester compound present in the recovered bis(2-hydroxyethyl)terephthalate acts as a factor that destroys the regularity of the final polymer during the subsequent polymerization process of polyester and polyester copolymer, thereby deteriorating the heat resistance characteristics of the final polymer, such as melting point (Tm), glass transition temperature (Tg), etc.
[0047] However, polyester resins and products made using the recycled bis(2-hydroxyethyl)terephthalate obtained by the depolymerization method according to the present invention can be polymerized into polymers without the occurrence of unnecessary structural defects as in the case of using unrecycled raw materials.
[0048] Depolymerization
[0049] According to the method of the present invention, since the waste polyester is pre-treated by pulverization and undergoes a multi-stage depolymerization reaction at a low temperature, the content of the glycol dimer (diethylene glycol) formed during the depolymerization reaction can be significantly reduced, thereby having the advantages of improving the purity of the finally obtained recovered bis(2-hydroxyethyl)terephthalate and minimizing the side reaction structure in the subsequent repolymerization into polyester.
[0050] According to one embodiment, the depolymerization includes depolymerizing the waste polyester through a first glycolysis reaction at a high temperature (180 to 200° C.) to obtain a first reactant; and depolymerizing the first reactant through a second glycolysis reaction at a low temperature (150 to 170° C.) to obtain a second reactant.
[0051] As is well known, glycolysis reaction refers to a chemical reaction in which polymer chains, etc., are decomposed by diols. The diols may include, for example, at least one selected from ethylene glycol, propylene glycol, and diethylene glycol.
[0052] A catalyst can be used in the glycolysis reaction. The catalyst can be a metal catalyst, such as a metal salt catalyst or a metal organic catalyst. Specifically, the catalyst can be an acetate, carbonate, oxide or hydroxide of a metal, and the metal can be an alkali metal, an alkaline earth metal or a transition metal.
[0053] As a specific example, the catalyst comprises a metal acetate or an anhydride or a hydride thereof. More specifically, the catalyst may be at least one selected from the group consisting of zinc acetate, sodium acetate, cobalt acetate and manganese acetate, or a hydrate or anhydride thereof.
[0054] The total weight of the added diol may be 1, 2 or 3 times or more of the weight of the waste polyester resin, and may be 7, 5 or 4 times or less. For example, the weight of the added diol may be 1 to 7 times, specifically, 2 to 5 times, more specifically, 3 to 4 times, relative to the weight of the waste polyester resin.
[0055] In addition, the weight of the added catalyst may be 0.01 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, or 0.3 parts by weight or more, and may also be 5 parts by weight or less, 1 part by weight or less, 0.7 parts by weight or less, 0.5 parts by weight or less, or 0.4 parts by weight or less, relative to 100 parts by weight of the waste polyester resin. For example, the weight of the added catalyst may be 0.1 parts by weight to 1 part by weight, specifically, 0.2 parts by weight to 0.7 parts by weight, relative to 100 parts by weight of the waste polyester resin. More specifically, the amount of the catalyst may be 0.2 parts by weight to 0.4 parts by weight relative to 100 parts by weight of the waste polyester.
[0056] The temperature during the first glycolysis reaction may be 170° C. or more, 180° C. or more, or 190° C. or more, and may be 205° C. or less, 200° C. or less, 195° C. or less, or 190° C. or less. For example, the temperature during the first glycolysis reaction may be 180° C. to 200° C., specifically, 180° C. to 195° C., more specifically, 180° C. to 190° C.
[0057] In addition, the temperature during the second glycolysis reaction may be 140° C. or more, 150° C. or more, or 160° C. or more, and may be 170° C. or less, or 160° C. or less. For example, the temperature during the second glycolysis reaction may be 150° C. to 170° C., specifically, 150° C. to 160° C., more specifically, 150° C. to 155° C.
[0058] From the time point when the appropriate temperature is reached, the time required for the first and second glycolytic reactions can be 1 hour or longer or 2 hours or longer, and can be 4 hours or shorter or 3 hours or shorter. For example, from the time point when the appropriate temperature is reached, the time required for the first and second glycolytic reactions can be 1 hour to 4 hours, specifically, 1 hour to 3 hours, more specifically, 1 hour to 2 hours.
[0059] As a specific example, the first glycolysis reaction may be performed at a temperature of 180° C. to 190° C. for 1 to 3 hours. In addition, the second glycolysis reaction may be performed at a temperature of 150° C. to 160° C. for 1 to 3 hours.
[0060] As an example, the first glycolysis reaction can be carried out in the presence of an acetic zinc anhydride catalyst. As a specific example, the first glycolysis reaction can be carried out at a temperature of 180°C to 200°C for 1 to 3 hours in the presence of an acetic zinc anhydride catalyst. More specifically, the amount of acetic zinc anhydride can be 0.2 to 0.4 parts by weight relative to 100 parts by weight of waste polyester. In addition, the second glycolysis reaction can be carried out at a temperature of 140 to 160°C for 1 to 3 hours when ethylene glycol is further added without adding an additional catalyst.
[0061] Cooling and filtration
[0062] The second reactant obtained by depolymerization can then be cooled and used in the next step.
[0063] For example, the cooling temperature may be 150°C or lower, 140°C or lower, 130°C or lower, 120°C or lower, 110°C or lower, 100°C or lower, and may also be 50°C or higher, 60°C or higher, 70°C or higher, 80°C or higher, or 90°C or higher.
[0064] As an example, cooling can be performed by a reduced pressure flash process. Specifically, the temperature of the second reactant can be reduced by applying a vacuum to evaporate ethylene glycol through a reduced pressure flash process.
[0065] For example, before the subsequent step, the second reactant may further undergo a step of cooling to 120° C. or less by reduced pressure flash distillation. More specifically, the temperature of the second reactant may be reduced to 110° C. or less or 100° C. or less by the reduced pressure flash distillation process.
[0066] The pressure condition of the reduced pressure flash process may be, for example, 200 Torr or less, 100 Torr or less, or 50 Torr or less, specifically, 10 Torr to 200 Torr, 10 Torr to 100 Torr, or 10 Torr to 50 Torr.
[0067] Thereafter, insoluble foreign matter can be removed from the cooled second reactant by filtration. As a specific example, before the ion exchange in step (3), a step of cooling the second reactant to 120° C. or less and adding a filter aid for filtration can be further performed. As a result, the fine particles and insoluble organic matter present in the second reactant can be filtered out by solid-liquid separation.
[0068] As the filter aid, known components such as diatomaceous earth, pearlite, asbestos powder, etc. can be used. For example, 0.1 to 2.0 parts by weight of the filter aid can be added to 100 parts by weight of the second reactant.
[0069] Since bis(2-hydroxyethyl)terephthalate (BHET) or oligomers obtained by depolymerization reaction exist in a solid form at room temperature, it is difficult to separate foreign matter at room temperature. Therefore, it is preferable to separate them under the temperature condition of 90° C. to 150° C., more specifically 110° C. to 150° C. In addition, if it is kept within the above temperature range, the removal of insoluble foreign matter can be promoted due to good fluidity.
[0070] Various methods and devices can be used to remove insoluble foreign matter by solid-liquid separation. For example, devices such as pressure filters, centrifugal separators, filter presses, and belt filter presses can be used. However, this is not limited to these, and any method that can separate foreign matter can be used.
[0071] Ion Exchange
[0072] The second reactant after depolymerization, cooling and filtering is subjected to ion exchange through an ion exchange resin to obtain a third reactant.
[0073] When it is subjected to ion exchange, ionic impurities present in the second reactant, particularly catalysts and foreign substances, can be removed.
[0074] As is well known, ion exchange resin refers to a resin or polymer used as an ion exchange medium. Ion exchange resins may include cation exchange resins, anion exchange resins, amphoteric ion exchange resins, chelating resins, and the like.
[0075] The cation exchange resin may include a strong acid cation exchange resin having a sulfonic acid group (-SO3H) and a weak acid cation exchange resin having a carboxyl group (-COOH). The anion exchange resin may include a strong basic anion exchange resin in the form of a quaternary ammonium salt and a weak basic anion exchange resin having primary to tertiary amino groups.
[0076] As a specific example, the ion exchange resin may include at least one selected from the group consisting of a strong acid cation exchange resin, a weak acid cation exchange resin, and a chelating resin.
[0077] According to one embodiment, the ion exchange is performed by adding an ion exchange resin to the second reactant.
[0078] The weight of the added ion exchange resin may be 1, 3 or 5 times or more of the weight of the catalyst added in the depolymerization reaction, and may be 20, 15, 10 or 8 times or less. For example, the weight of the added ion exchange resin may be 1 to 20 times, specifically, 3 to 15 times, more specifically, 5 to 8 times, relative to the weight of the catalyst added in the depolymerization reaction.
[0079] In addition, the weight of the ion exchange resin added may be 1 part by weight or more, 3 parts by weight or more, or 5 parts by weight or more, and may be 50 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, or 7 parts by weight or less, relative to 100 parts by weight of the waste polyester resin used in the depolymerization reaction.
[0080] As a specific example, the ion exchange resin may be used in an amount of 1 to 20 parts by weight relative to 100 parts by weight of the waste polyester.
[0081] According to another embodiment, the ion exchange is performed by using a column containing an ion exchange resin.
[0082] Specifically, the column may be filled with ion exchange resin particles, and ion exchange may be performed while the second reactant passes through the column.
[0083] The particle size of the ion exchange resin particles may be, for example, 0.3 mm to 1.5 mm, more specifically 0.6 mm to 0.9 mm.
[0084] The temperature of ion exchange may be, for example, 140°C or less, 130°C or less, 120°C or less, 110°C or less, 100°C or less, and may be 50°C or more, 60°C or more, 70°C or more, 80°C or more, or 90°C or more.
[0085] Removal of unreacted diol
[0086] Unreacted diol is removed from the third reactant by distillation to obtain a fourth reactant.
[0087] Since unreacted diol still remains in the depolymerization product after filtration in the previous step, it is necessary to remove it from the reactants before the next step.
[0088] In addition, in order to realize an economical depolymerization method, a step of recovering unreacted diols is required, that is, diols previously used in depolymerization, such as ethylene glycol, propylene glycol, diethylene glycol, etc., which remain without participating in the glycolysis reaction, can be recovered and reused.
[0089] The distillation to remove the unreacted diol can be carried out, for example, by vacuum distillation. A glass distillation apparatus or a rotary evaporator can be used for this purpose.
[0090] Since the vacuum distillation for removing the unreacted diol is carried out at a temperature of 150° C. or lower, the purity of BHET can be improved by further reducing the formation of diethylene glycol and impurities derived therefrom. For example, the vacuum distillation for removing the unreacted diol can be carried out at a temperature below 150° C., below 130° C., or below 120° C., and above 80° C., above 90° C., above 100° C., or above 110° C. Specifically, the temperature when the unreacted diol is removed by distillation can be 80° C. to 190° C. or 90° C. to 150° C. As a more specific example, the unreacted diol can be removed by distillation at a temperature of 100° C. to 130° C.
[0091] The pressure during the distillation process when removing unreacted diol may be, for example, 0.1 Torr to 200 Torr, more specifically, 0.5 Torr to 30 Torr.
[0092] Distillation
[0093] The fourth reactant from which unreacted diol has been removed is distilled to obtain crude bis(2-hydroxyethyl)terephthalate.
[0094] Various methods can be used for distillation, and distillation methods that separate the mixture into thin films to increase its surface area in contact with the heat source can be used.
[0095] For example, the distillation can be carried out by thin film evaporation, falling film evaporation or short path evaporation. For this purpose, a thin film evaporator, a falling film evaporator and a short path evaporator can be used respectively.
[0096] As a specific example, distillation can be performed by thin film evaporation to obtain bis(2-hydroxyethyl)terephthalate. Specifically, the mixture supplied to the evaporator of the thin film evaporator forms a thin film on the inner wall of the thin film evaporator by a wiper rotor. Then, distillation is performed under appropriate temperature conditions by heating. In addition, a condenser for recovering evaporated materials can be provided inside the thin film evaporator.
[0097] Thin film evaporation can be performed by short-path evaporation. Because of this short path and the short residence time of thin film evaporation, and the ability to use high vacuum for vacuum distillation, it is possible to separate high boiling point or high molecular weight materials that are difficult to separate by other distillation methods, while minimizing the thermal changes of the reactants. In addition, if the pressure inside the thin film evaporator is reduced, there is an advantage that the vapor pressure of the material is reduced, which allows evaporation to be performed at a temperature below its original boiling point.
[0098] As a specific example, the fourth reactant is supplied to the short path and thin film evaporator, and the wiper for forming the thin film is rotated at a speed of 300 rpm or more. As a result, the vaporized material and the non-vaporized material can be separated from each other.
[0099] During thin film evaporation, the internal film temperature of the upper thin film evaporation device can be, for example, 100°C or higher, 110°C or higher, 120°C or higher, or 125°C or higher, and can be 250°C or lower, 200°C or lower, 150°C or lower, or 135°C or lower, specifically, 150°C to 250°C, 190°C to 250°C, or 180°C to 220°C.
[0100] In addition, during thin film evaporation, the internal pressure of the upper thin film evaporation device may be, for example, 0.005 Torr to 5.0 Torr, specifically, 0.05 Torr to 5.0 Torr, 0.05 Torr to 1.5 Torr, or 0.05 Torr to 1 Torr. More specifically, distillation may be performed by thin film evaporation at a pressure of 0.05 Torr to 0.4 Torr to obtain crude bis(2-hydroxyethyl)terephthalate.
[0101] Adsorption-crystallization
[0102] The crude bis(2-hydroxyethyl)terephthalate is subjected to an adsorption-crystallization step to obtain high-purity, high-quality recovered bis(2-hydroxyethyl)terephthalate.
[0103] For example, adsorption-crystallization can be performed by adding an adsorbent using water as a solvent, filtering, and crystallizing.
[0104] Various solvents can be used for adsorption crystallization, but preferably a solvent capable of dissolving bis(2-hydroxyethyl)terephthalate is used as a solvent. As a specific example, in order to obtain the final reactant, water is added as a solvent to crude bis(2-hydroxyethyl)terephthalate, which is dissolved by heating, and an adsorbent is added thereto, and then the solution obtained by filtration is cooled for crystallization and finally filtered. As a result, highly pure recovered bis(2-hydroxyethyl)terephthalate can be obtained.
[0105] The amount of water added may be 100 to 500 parts by weight, specifically 200 to 400 parts by weight, and more specifically 300 to 350 parts by weight, relative to 100 parts by weight of crude bis(2-hydroxyethyl)terephthalate.
[0106] In addition, the dissolution temperature may be 50°C to 95°C, specifically, 60°C to 85°C, and more specifically, 70°C to 75°C.
[0107] The added adsorbent can be used to adsorb and remove other foreign matter. The added amount can be 0.1 to 3 parts by weight relative to 100 parts by weight of crude bis(2-hydroxyethyl)terephthalate. The type and form of the adsorbent are not particularly limited. For example, activated carbon can be used.
[0108] Recycled bis(2-hydroxyethyl)terephthalate
[0109] Bis(2-hydroxyethyl)terephthalate (BHET) obtained by depolymerization of waste polyester is referred to as recycled bis(2-hydroxyethyl)terephthalate (recycled BHET, or r-BHET), which needs to be understood to be different from pure BHET compound.
[0110] Specifically, the recovered BHET may contain reagents or solvents used in various chemical steps during the depolymerization of waste polyester, or byproducts formed by side reactions therewith. Even after several rounds of purification, these impurities may still remain in trace amounts. Therefore, the recovered BHET, in addition to BHET as the main component, generally contains trace amounts of organic and inorganic impurities. Therefore, the recovered BHET can also be regarded as a "composition" containing two or more components, i.e., a "BHET composition".
[0111] Specifically, the recovered BHET may contain trace amounts of heterogeneous organic components, such as BHET analogs such as monohydroxyethyl terephthalate (MHET), BHET dimers, BHET trimers, by-products such as diethylene glycol esters, metal ions as inorganic components, and residual solvent components, in addition to BHET as the main component.
[0112] However, the recovered BHET finally obtained according to the present invention has high purity, contains a certain level or less of organic impurities, especially diethylene glycol and its derived by-products (DEG esters, etc.) or other oligomers and inorganic substances, and it has excellent color quality.
[0113] This can be confirmed by analyzing the final product obtained by the above method with high performance liquid chromatography (HPLC) and calculating the relative ratio between the peak areas of each component. Specifically, the content of each component can be obtained by measuring the fraction (%) of the peak area in the spectrum obtained using high performance liquid chromatography in the total peak area.
[0114] For example, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of bis(2-hydroxyethyl)terephthalate of 90% or more, 93% or more, or 95% or more when measured by HPLC.
[0115] According to one embodiment, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of bis(2-hydroxyethyl)terephthalate of 96% or more when measured by HPLC. Specifically, the peak area fraction of bis(2-hydroxyethyl)terephthalate may be 96.5% or more, 97% or more, 97.5% or more, or 98% or more.
[0116] In addition, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of organic impurities of less than 5% in total measured by HPLC, specifically, less than 4%, less than 3%, less than 2%, less than 1% or less than 0.7% in total.
[0117] According to one embodiment, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of diethylene glycol ester compounds of less than 2% in total when measured by HPLC. Specifically, the peak area fraction of diethylene glycol ester compounds may be less than 1.5%, less than 1%, less than 0.8% or less than 0.7% in total.
[0118] The diethylene glycol ester compound may be, for example, a condensate between an aromatic dicarboxylic acid such as terephthalic acid and diethylene glycol. As another example, the diethylene glycol ester compound may be a condensate between an aromatic dicarboxylic acid other than diethylene glycol such as terephthalic acid and a diol (e.g., ethylene glycol). As a specific example, the diethylene glycol ester compound may include at least one of 2-hydroxyethyl [2-(2-hydroxyethoxy)ethyl] terephthalate and bis [2-(2-hydroxyethoxy)ethyl] benzene-1,4-dicarboxylate.
[0119] In addition, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method can have a peak area fraction of oligomers of 3% or less in total when measured by HPLC. This is a very excellent level in terms of purity and quality compared to the 10% to 20% of oligomeric materials present in the product obtained by depolymerization by conventional methods.
[0120] Specifically, when measured by HPLC, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of BHET dimer of less than 3%, less than 2%, less than 1%, or less than 0.7%. In addition, when measured by HPLC, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a peak area fraction of BHET trimer of less than 1%, less than 0.5%, less than 0.3%, less than 0.1%, or 0%.
[0121] In addition, the final product may also contain impurities having a structure similar to bis(2-hydroxyethyl)terephthalate. For example, it may contain at least one selected from the group consisting of monohydroxyethyl terephthalate (MHET), bis(2-hydroxyethyl)terephthalate, and monohydroxyethylethoxy terephthalate. When measured by HPLC, the impurities having a structure similar to bis(2-hydroxyethyl)terephthalate may have a peak area fraction of less than 3%, less than 2%, less than 1%, or less than 0.5%.
[0122] In addition, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method may have a yellowness index (YID) of 3.0 or less measured with a spectrophotometer. Specifically, the yellowness index may be 2.5 or less, 2.0 or less, 1.5 or less, or 1.0 or less.
[0123] In addition, the recovered bis(2-hydroxyethyl)terephthalate prepared by the above method can have a total content of less than 5 ppm of inorganic substances measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES). Specifically, the total content of inorganic substances can be less than 3 ppm, less than 1 ppm or close to 0 ppm.
[0124] Embodiments of the invention
[0125] The present invention will be described in detail below with reference to embodiments. However, these embodiments are for illustrative purposes only, and the present invention is not limited thereto.
[0126] Example 1
[0127] Into a first reactor made of stainless steel (SUS), 1,000 g of waste polyester resin pulverized to a particle size of 4 mm or less, 2,000 g of ethylene glycol and 3.5 g of acetic zinc anhydride were charged. The temperature inside the reactor was raised to 180° C., and depolymerization (first glycolysis reaction) was performed for 2 hours.
[0128] The reactant (first reactant) thus obtained was transferred to a second reactor and cooled to 150° C. 2,000 g of ethylene glycol was further added thereto, and depolymerization (second glycolysis reaction) was performed for 2 hours while the reactor temperature was maintained at 150° C.
[0129] The reactant thus obtained (second reactant) was cooled to 120° C. by flash evaporation under reduced pressure, and 16 g of a filter aid (Celite TM 545), followed by pressure filtration for solid-liquid separation.
[0130] The separated liquid reactant was passed through a column filled with an ion exchange resin (BC107(H) of Bonlite) to remove ion impurities to obtain a mixture containing bis(2-hydroxyethyl)terephthalate and ethylene glycol (third reactant).
[0131] The mixture (third reactant) was transferred to a 10-liter distillation apparatus and subjected to vacuum distillation at 130° C. to recover unreacted ethylene glycol.
[0132] The reactant (fourth reactant) from which ethylene glycol had been removed was subjected to thin film evaporation at 220° C. and 0.08 torr in a thin film evaporator (VTA's VKL70-4S) to obtain 1,040 g of a product from which dimers or higher oligomers had been removed. Thereafter, for adsorption crystallization, 1,040 g of the above product and 3,120 g of distilled water were charged into a 20-liter glass reactor, dissolved at a temperature of 70° C., and then 5.2 g of activated carbon was added thereto, followed by stirring for 30 minutes and filtering. The filtrate was cooled to room temperature for crystallization, filtered, and dried in a vacuum oven. As a result, 990 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained.
[0133] Example 2
[0134] 980 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Example 1, except that the first glycolysis reaction was performed at 180° C. for 1 hour.
[0135] Example 3
[0136] 985 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedure as in Example 1 except that 1,000 g of waste fibers was used as a raw material of waste polyester.
[0137] Example 4
[0138] 992 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedure as in Example 1 except that 1,000 g of the waste banner was used as a raw material of the waste polyester.
[0139] Example 5
[0140] 1,050 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedure as in Example 1 except that the adsorption crystallization step was not performed after the thin film evaporation.
[0141] Comparative Example 1
[0142] Into a reactor made of stainless steel (SUS), 1,000 g of waste polyester resin having a particle size of 4 mm or less, 4,000 g of ethylene glycol and 3.5 g of acetic zinc anhydride are charged. The temperature in the reactor is raised to 196° C., and depolymerization (glycolysis reaction) is performed for 4 hours. The resulting reactant is cooled to 30° C., and bis(2-hydroxyethyl)terephthalate is crystallized for 2 hours. The slurry of bis(2-hydroxyethyl)terephthalate and ethylene glycol thus obtained is subjected to solid-liquid separation in a centrifuge. The bis(2-hydroxyethyl)terephthalate obtained by centrifugation is washed twice with a sufficient amount of distilled water, and the residual solvent is removed in an oven to obtain about 1,010 g of a final product containing bis(2-hydroxyethyl)terephthalate.
[0143] Comparative Example 2
[0144] About 1,000 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Comparative Example 1, except that the glycolysis reaction was performed at 210°C.
[0145] Comparative Example 3
[0146] 1,020 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Example 1, except that the first glycolysis reaction was performed at 196° C. for 4 hours, and neither the second glycolysis reaction nor the adsorption crystallization was performed.
[0147] Comparative Example 4
[0148] 730 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Example 1, except that the first glycolysis reaction was performed at 150° C. for 10 minutes and the second glycolysis reaction was performed at 190° C. for 1 hour and 30 minutes.
[0149] In this case, since the temperature of the first glycolysis reaction is low, a large amount of unreacted waste PET residue is filtered in the final reaction, and the filtration time exceeds 10 hours, the method has problems, and the final yield is also reduced.
[0150] Comparative Example 5
[0151] About 1,050 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Example 1, except that the first glycolysis reaction was performed at 210°C and the second glycolysis reaction was performed at 250°C.
[0152] Comparative Example 6
[0153] About 995 g of a final product containing bis(2-hydroxyethyl)terephthalate was obtained by the same procedures as in Example 1 except that the unreacted diol was recovered at 160°C.
[0154] Test Case
[0155] The products of Examples and Comparative Examples (recovered bis(2-hydroxyethyl)terephthalate) were subjected to the following tests. The results are summarized in Table 1 below.
[0156] (1) Composition - High Performance Liquid Chromatography (HPLC)
[0157] About 0.01 g of a sample was diluted in about 20 ml of methanol and then measured by HPLC.
[0158] -Model: Waters e2695
[0159] - Column: C18 (4.6×250 mm), 5 μm
[0160] -UV detector: 242nm
[0161] -Injection volume: 10μl
[0162] -Eluent (gradient) A: H2O+H3PO4, B: acetonitrile
[0163] (2) Residual solvents - gas chromatography (GC)
[0164] About 0.1 g of a sample was diluted in about 10 ml of CHCl 3 , treated with a 0.45 μm filter, and then measured by GC.
[0165] -Model: Agilent 7890B
[0166] - Column: DB-624 (30m×0.25mm×1.4μm)
[0167] - Oven temperature: 60℃(2min)-10℃ / min-200℃(0min)-20℃ / min-260℃(5min)
[0168] - Injector temperature: 250℃
[0169] -Detector temperature: 250℃
[0170] -Flow rate: 1.5ml / min (N2), split ratio: 1 / 50
[0171] (3) Melting point-Differential Scanning Calorimetry (DSC)
[0172] Melting points (mp) were measured using a differential scanning calorimeter (DSC, TA Instruments Q20) with heating from 30°C to 280°C at a rate of 10°C / min.
[0173] (4) Inorganic substances - Inductively coupled plasma atomic emission spectrometry (ICP-AES)
[0174] 0.3 g of the sample was treated with ultrasonic waves and diluted with ultrapure water. The content (ppm) of inorganic substances was measured using ICP-AES (Agilent 5100 model) (detection limit: 5 ppm).
[0175] (5) Yield
[0176] The weight percentage of bis(2-hydroxyethyl)terephthalate actually obtained in Examples and Comparative Examples was calculated based on the maximum weight of bis(2-hydroxyethyl)terephthalate obtained from 1,000 g of polyethylene terephthalate through a glycolysis reaction.
[0177] (6) Yellowness Index (YID)
[0178] The sample was dissolved in dimethylformamide (DMF) at a concentration of 25 wt% at room temperature (23°C) to prepare a solution. For the solution, the transmission data was obtained using Hunterlab's Color Flex EZ using Illuminant D65 at a 2° observer angle. The YID value was calculated using the color analyzer in the software.
[0179] [Table 1]
[0180]
[0181] As can be seen from the above table, in the products obtained in Examples 1 to 5, the proportion of BHET is high, no inorganic impurities are observed, the YID value is low, and the content of DEG-derived esters can be minimized. The polyester resin polymerized from the high-purity recovered BHET has excellent thermal properties such as glass transition temperature, melting point and crystallization temperature; therefore, it can reproduce the structural regularity, molecular weight and excellent thermal properties of the original polyester resin.
[0182] In contrast, the products obtained in Comparative Examples 1 and 5 have problems in that they contain a large amount of dimer or DEG-derived ester, have poor color quality due to a high yellowness index (YID), or have a significantly low yield.
Claims
1. A method for preparing recovered bis(2-hydroxyethyl)terephthalate, comprising: (1) depolymerizing the waste polyester through a first glycolysis reaction at a temperature of 180° C. to 200° C. to obtain a first reactant; (2) depolymerizing the first reactant through a second glycolysis reaction at a temperature of 150° C. to 170° C. to obtain a second reactant; (3) performing ion exchange on the second reactant through an ion exchange resin to obtain a third reactant; (4) removing unreacted diol from the third reactant by distillation at a temperature of 150° C. or less to obtain a fourth reactant; and (5) The fourth reactant is distilled to obtain crude bis(2-hydroxyethyl)terephthalate.
2. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, wherein: The waste polyester is in a granular or fibrous form, and has a particle size of 4 mm or less.
3. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, wherein: The first glycolysis reaction in step (1) is carried out in the presence of a catalyst, and the catalyst comprises a metal acetate or its anhydride or its hydride, and the amount of the catalyst is 0.2 to 0.4 parts by weight relative to 100 parts by weight of the waste polyester resin.
4. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, further comprising, before the ion exchange of step (3), cooling the second reactant to 120°C or less and filtering after adding a filter aid.
5. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, further comprising removing insoluble foreign matter in the second reactant by filtration before the ion exchange in step (3).
6. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, wherein: The ion exchange resin used in step (3) is 1 to 20 parts by weight relative to 100 parts by weight of the waste polyester, and comprises at least one selected from the group consisting of a strongly acidic cation exchange resin, a weakly acidic cation exchange resin and a chelating resin.
7. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, wherein: The distillation for removing unreacted diol in step (4) is carried out at a temperature of 100°C to 130°C.
8. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, wherein: The crude bis(2-hydroxyethyl)terephthalate obtained by the distillation is carried out by thin film evaporation at a pressure of 0.05 to 0.4 torr.
9. The method for preparing recovered bis(2-hydroxyethyl)terephthalate according to claim 1, further comprising, after the distillation of step (5), adsorption-crystallization of the crude bis(2-hydroxyethyl)terephthalate, wherein the adsorption-crystallization is performed by adding an adsorbent using water as a solvent, filtering and crystallizing.
10. A recovered bis(2-hydroxyethyl)terephthalate prepared by the method according to claim 1, wherein the peak area fraction of bis(2-hydroxyethyl)terephthalate is 96% or more and the peak area fraction of diethylene glycol ester compounds is less than 2% in total when measured by high performance liquid chromatography (HPLC).
11. The recovered bis(2-hydroxyethyl)terephthalate according to claim 10, wherein The recovered bis(2-hydroxyethyl)terephthalate has a peak area fraction of oligomers of 3% or less in total when measured by high performance liquid chromatography.
12. The recovered bis(2-hydroxyethyl)terephthalate according to claim 10, wherein The recovered bis(2-hydroxyethyl)terephthalate has a yellowness index (YID) of 3.0 or less measured with a spectrophotometer.
13. The recovered bis(2-hydroxyethyl)terephthalate according to claim 10, wherein The recovered bis(2-hydroxyethyl)terephthalate has a total content of inorganic substances of less than 5 ppm as measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES).
Citation Information
Cited By
Method for efficiently depolymerizing waste PET polyester at low temperature
CN120590682A