Composition
By bonding a specific amount of chlorine and fluorine atoms in the aromatic polyether and combining it with discontinuous carbon fibers, the composition formed solves the problems of poor reinforcement effect of discontinuous carbon fibers and increased viscosity of the composition in the existing technology, achieving It achieves the lightweight effect of high tensile strength and good kneadability.
Patent Information
- Application Number
- CN202380024445.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for the existing technology to effectively exert the reinforcing effect brought by discontinuous carbon fibers, and the increased viscosity of the composition results in poor kneadability and lack of lightweight effect.
By bonding specific amounts of chlorine and fluorine atoms in an aromatic polyether and combining it with discontinuous carbon fibers, the resulting composition is based on 4,4'-dichlorobenzophenone and 4,4'-difluoro As a monomer component, benzophenone adjusts the chemical structure of the composition to improve tensile strength and kneadability.
It is possible to significantly improve the tensile strength and kneadability of the composition without increasing the amount of discontinuous carbon fiber, thereby achieving the effect of lightweighting the composition.
Smart Images

Figure CN118786181A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to compositions.
[0002] Specifically, the present invention relates to a composition capable of effectively exerting the reinforcing effect of discontinuous carbon fibers. Background Art
[0003] Patent Document 1 discloses that a specific aromatic polyether produced by allowing a component having a specific polymerization catalytic action to exist in a reaction system is mixed with a reinforcing material or filler such as glass fiber, carbon fiber, aramid fiber, calcium carbonate, or calcium silicate.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 64-0651.29 Summary of the invention
[0007] However, in the prior art represented by Patent Document 1, room for further improvement has been found from the viewpoint of effectively exerting the reinforcing effect of the discontinuous carbon fibers.
[0008] One of the objects of the present invention is to provide a composition that can effectively exert the reinforcing effect of discontinuous carbon fibers.
[0009] The present inventors have conducted intensive studies and, as a result, have found that when discontinuous carbon fibers are blended with specific aromatic polyethers, the reinforcing effect of the discontinuous carbon fibers is effectively exerted, thereby completing the present invention.
[0010] According to the present invention, the following compositions can be provided.
[0011] 1. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), and the amount of chlorine atoms bonded to the aromatic polyether is 10 to 10000 ppm by mass.
[0012]
Chemical formula 1
[0013]
[0014] 2. The composition according to 1, wherein the amount of fluorine atoms bonded to the aromatic polyether is 10 to 10,000 ppm by mass.
[0015] 3. The composition according to 1 or 2, comprising an aromatic polyether formed using 4,4'-dichlorobenzophenone as a monomer component.
[0016] 4. The composition according to any one of 1 to 3, wherein the aromatic polyether comprises a repeating unit represented by the following formula (3).
[0017]
Chemical formula 2
[0018]
[0019] 5. The composition according to any one of 1 to 4, wherein the average fiber length of the discontinuous carbon fibers is 0.5 to 20 mm.
[0020] 6. The composition according to any one of 1 to 5, wherein the content of the discontinuous carbon fiber is 5 to 100 parts by mass based on 100 parts by mass of the aromatic polyether.
[0021] 7. The composition according to any one of 1 to 6, which has a tensile strength of 2.80 times or more the tensile strength of the aromatic polyether alone.
[0022] 8. The composition according to any one of 1 to 6, which has a tensile strength of 2.35 to 5.00 times the tensile strength of the aromatic polyether alone.
[0023] 9. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), and the total chlorine content in the aromatic polyether is 10 to 10000 ppm by mass.
[0024]
Chemical formula 3
[0025]
[0026] 10. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), and the ratio of the total chlorine content in the aromatic polyether to the total chlorine content in the aromatic polyether and the total fluorine content in the aromatic polyether is 40 to 100% by mass.
[0027]
Chemical formula 4
[0028]
[0029] 11. The composition according to 9 or 10, wherein the total chlorine content in the aromatic polyether is 100 to 10,000 ppm by mass, and the total fluorine content in the aromatic polyether is 100 to 2,000 ppm by mass.
[0030] 12. The composition according to any one of 9 to 11, wherein the aromatic polyether comprises a repeating unit represented by the following formula (3).
[0031]
Chemical formula 5
[0032]
[0033] 13. The composition according to any one of 9 to 12, wherein the average fiber length of the discontinuous carbon fibers is 0.5 to 20 mm.
[0034] 14. The composition according to any one of 9 to 13, wherein the content of the discontinuous carbon fiber is 5 to 100 parts by mass based on 100 parts by mass of the aromatic polyether.
[0035] 15. The composition according to any one of 9 to 14, which has a tensile strength of 2.80 times or more the tensile strength of the aromatic polyether alone.
[0036] 16. The composition according to any one of 9 to 14, which has a tensile strength of 2.35 to 5.00 times the tensile strength of the aromatic polyether alone.
[0037] According to the present invention, a composition capable of effectively exerting the reinforcing effect of discontinuous carbon fibers can be provided.
[0038] Thus, for example, when a certain level of strength is imparted to the composition, the effect of reducing the amount of discontinuous carbon fibers compared to the prior art can be obtained. By reducing the amount of discontinuous carbon fibers, the viscosity increase of the composition can be suppressed and the kneading property can be improved, and the effect of making the composition lighter can also be obtained. DETAILED DESCRIPTION
[0039] Hereinafter, the composition of the present invention will be described in detail.
[0040] In addition, in this specification, "x to y" represents a numerical range of "x or more and y or less." The upper limit value and the lower limit value described in the numerical range can be arbitrarily combined.
[0041] A composition according to one embodiment of the present invention (also referred to as the first embodiment) comprises an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), and the amount of chlorine atoms bonded to the aromatic polyether is 10 to 10,000 ppm by mass.
[0042]
Chemical formula 6
[0043]
[0044] According to the composition of this aspect, it is possible to obtain an effect in which the reinforcing effect of the discontinuous carbon fibers can be effectively exerted.
[0045] Thus, for example, when a certain level of strength is imparted to the composition, the effect of reducing the amount of discontinuous carbon fibers compared to the prior art can be obtained. By reducing the amount of discontinuous carbon fibers, the viscosity increase of the composition can be suppressed and the kneading property can be improved, and the effect of making the composition lighter can also be obtained.
[0046] (Aromatic polyether)
[0047] Hereinafter, the method for measuring the amount of chlorine atoms bonded in the aromatic polyether (Cl-1), the amount of chlorine atoms contained as free components in the aromatic polyether (Cl-2, also referred to as "inorganic chlorine content"), and the total amount of these chlorine atoms (Cl-3, also referred to as "total chlorine content in the aromatic polyether") will be described. In addition, the method for measuring the amount of fluorine atoms bonded in the aromatic polyether (F-1), the amount of fluorine atoms contained as free components in the aromatic polyether (F-2, also referred to as "inorganic fluorine content"), and the total amount of these fluorine atoms (F-3, also referred to as "total fluorine content in the aromatic polyether") will be described. In addition, the method for measuring the amount of potassium atoms and the amount of sodium atoms contained as free components in the aromatic polyether will be described.
[0048] <Calculation of the Amount of Chlorine Atoms Bonded in Aromatic Polyether (Cl-1)>
[0049] a. The total chlorine content (mass ppm) (Cl-3) was calculated from the result of measuring the total chlorine amount (*1: described later) of the aromatic polyether.
[0050] b. For aromatic polyethers, the potassium content (mass ppm) is calculated from the measured value of the potassium amount (*2: described later), and the inorganic chlorine content (mass ppm) (Cl-2) is calculated by assuming that the inorganic chlorine (chlorine atoms not bonded to the aromatic polyether) is contained in an amount equimolar to potassium.
[0051] c. The amount of chlorine atoms bonded to the aromatic polyether (mass ppm) (Cl-1) was calculated by subtracting the content of inorganic chlorine (mass ppm) (Cl-2) from the content of total chlorine (mass ppm) (Cl-3).
[0052] <Calculation of the Amount of Fluorine Atoms Bonded to Aromatic Polyether (F-1)>
[0053] a. The total fluorine content (mass ppm) was calculated from the result of measuring the total fluorine content (*1: described later) of the aromatic polyether (F-3).
[0054] b. For the aromatic polyether, the sodium content (mass ppm) is calculated from the measured value of the sodium amount (*2: described later), and the inorganic fluorine content (mass ppm) is calculated (F-2) assuming that the inorganic fluorine (fluorine atoms not bonded to the aromatic polyether) is contained in an amount equal in mole to that of sodium.
[0055] c. The amount of fluorine atoms bonded to the aromatic polyether (mass ppm) (F-1) was calculated by subtracting the content of inorganic fluorine (mass ppm) (F-2) from the content of total fluorine (mass ppm) (F-3).
[0056] (*1) Determination method of total chlorine (Cl-3) and total fluorine (F-3) in aromatic polyethers
[0057] The sample (aromatic polyether) is introduced into a combustion furnace and burned in a combustion gas containing oxygen. After the generated gas is captured in an absorbent, the absorbent is separated and quantified using an ion chromatograph. The quantitative value is obtained based on a standard curve prepared based on a reference of known concentration. The measurement conditions are shown below.
[0058] <Sample Combustion>
[0059] Combustion device: AQF-2100H manufactured by Nittoseiko Analytech Co., Ltd.
[0060] Combustion furnace set temperature: front section 800, rear section 1100℃
[0061] Argon flow rate: 400ml / min
[0062] Oxygen flow rate: 200ml / min
[0063] Absorbent: Hydrogen peroxide
[0064] <Ion Chromatography>
[0065] Analytical device: Integrion manufactured by Thermo Fisher Scientific Co., Ltd.
[0066] Column: A guard column (Dionex IonPac AG12A) and a separation column (Dionex IonPac AS12A) were connected and used (both columns were manufactured by Thermo Fisher Scientific)
[0067] Eluent: Na2CO3 (2.7mmol / 1) + NaHCO3 (0.3mmol / 1)
[0068] Flow rate: 1.5ml / min
[0069] Column temperature: 30°C
[0070] Measurement mode: Suppression mode
[0071] Detector: Conductivity detector
[0072] (*2) Method for measuring the amount of potassium and sodium in aromatic polyethers (the amount of potassium atoms and the amount of sodium atoms contained as free components in aromatic polyethers)
[0073] The contents of potassium atoms (K) and sodium atoms (Na) in the aromatic polyether were determined by ICP emission spectrometry. The aromatic polyether was pretreated according to the following steps. Na was measured at 589.592 nm, and K was measured at 766.481 nm.
[0074] 1 g of a sample was weighed in a platinum dish, concentrated sulfuric acid was added thereto, and then heated to perform a carbonization treatment. Then, the platinum dish was placed in an electric furnace and ashing treatment was performed at 550° C. for 12 hours.
[0075] After the ashing treatment, hydrochloric acid is added, and then the mixture is heated. After cooling, the mixture is fixed to volume with ultrapure water. It should be noted that, in the case where the sample contains an inorganic filler (non-continuous carbon fiber), after the ashing treatment, hydrofluoric acid is added, and then the mixture is heated to dry solid. After cooling, hydrochloric acid is added, and then the mixture is heated. After cooling, the mixture is fixed to volume with ultrapure water.
[0076] The quantitative value is obtained based on a standard curve prepared from a reference of known concentration. The hydrochloric acid concentration of the standard curve solution is the same as that of the sample solution.
[0077] It should be noted that, regarding the calculation of the amount of chlorine atoms (mass ppm) (Cl-1) bonded in the aromatic polyether and the amount of fluorine atoms (mass ppm) (F-1) bonded in the aromatic polyether, when 4,4'-difluorobenzophenone and 4,4'-dichlorobenzophenone, which are monomers (reactants) used in the synthesis of the aromatic polyether, remain in the aromatic polyether, the amount of fluorine atoms contained as 4,4'-difluorobenzophenone and the amount of chlorine atoms contained as 4,4'-dichlorobenzophenone in the aromatic polyether are quantitatively determined by the following method to exclude the influence thereof.
[0078] First, the solid sample (aromatic polyether) is crushed with a stirrer, washed with acetone and water in sequence, and dried with an explosion-proof dryer at 180°C. It should be noted that when the reaction mixture (product) immediately after the reaction to generate the aromatic polyether is used as a sample, after the reaction is completed, the product is cooled and solidified to prepare the above-mentioned solid sample. The stirrer used is not particularly limited, and for example, 7010HS manufactured by Warling Company can be used.
[0079] Next, about 1 g of the dried sample was weighed in an eggplant-shaped flask, 100 ml of cyclohexanone and a boiling stone were added thereto, and the mixture was heated under reflux for 1 hour using a mantle heater. After cooling to room temperature, the solid content was removed by filtration.
[0080] Next, the obtained solution is measured by gas chromatography, thereby calculating the amount (mass ppm) of 4,4'-difluorobenzophenone and the amount (mass ppm) of 4,4'-dichlorobenzophenone in the sample. Here, the amount (mass ppm) of 4,4'-difluorobenzophenone and the amount (mass ppm) of 4,4'-dichlorobenzophenone in the sample are obtained based on a standard curve prepared based on a reference with a known concentration. The measurement conditions of gas chromatography are shown below.
[0081] <Gas Chromatography Measurement Conditions>
[0082] Analytical device: Agilent Technologies 8890
[0083] GC column: Agilent Technologies DB-HeavyWAX (length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm)
[0084] Inlet temperature: 250
[0085] Oven temperature: 250℃ (constant)
[0086] Flow rate: 1 ml / min
[0087] Injection volume: 1μl
[0088] Split ratio: 40:1
[0089] Detector: FID
[0090] Detector temperature: 250
[0091] The amount (mass ppm) of fluorine atoms contained as 4,4′-difluorobenzophenone and the amount (mass ppm) of chlorine atoms contained as 4,4′-dichlorobenzophenone in the aromatic polyether were converted by the following calculation formula.
[0092] The amount of fluorine atoms contained as 4,4'-difluorobenzophenone in the aromatic polyether (mass ppm) = the amount of 4,4'-difluorobenzophenone in the sample (mass ppm) ÷ 218.20 (molecular weight of 4,4'-difluorobenzophenone) × 19.00 (atomic weight of fluorine) × 2 The amount of chlorine atoms contained as 4,4'-dichlorobenzophenone in the aromatic polyether (mass ppm) = the amount of 4,4'-dichlorobenzophenone in the sample (mass ppm) ÷ 251.11 (4,4'-dichlorobenzophenone) If the amount of fluorine atoms contained as 4,4'-difluorobenzophenone and the amount of chlorine atoms contained as 4,4'-dichlorobenzophenone in the aromatic polyether (mass ppm) are both less than the quantitative lower limit of 100 mass ppm, then there is no influence on the calculation results of the amount of fluorine atoms bonded in the aromatic polyether (F-1) and the amount of chlorine atoms bonded in the aromatic polyether (Cl-1) (the influence can be ignored).
[0093] When the amount (mass ppm) of fluorine atoms contained as 4,4'-difluorobenzophenone in the aromatic polyether (F-4) is 100 mass ppm or more, the amount (mass ppm) of fluorine atoms bonded in the aromatic polyether (F-1) can be calculated by subtracting the content (mass ppm) of inorganic fluorine (F-2) from the total fluorine content (mass ppm) (F-3) and further subtracting the amount (mass ppm) of fluorine atoms contained as 4,4'-difluorobenzophenone (F-4).
[0094] When the amount (mass ppm) of chlorine atoms contained as 4,4'-dichlorobenzophenone in the aromatic polyether (Cl-4) is 100 mass ppm or more, the amount (mass ppm) of chlorine atoms bonded in the aromatic polyether (F-1) can be calculated by subtracting the content (mass ppm) of inorganic chlorine (Cl-2) from the total chlorine content (mass ppm) (Cl-3) and further subtracting the amount (mass ppm) of chlorine atoms contained as 4,4'-dichlorobenzophenone (Cl-4).
[0095] In one embodiment, the amount of chlorine atoms bonded in the aromatic polyether (Cl-1) is 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 500 mass ppm or more, 1000 mass ppm or more, or 2000 mass ppm or more, and is 10000 mass ppm or less, 6000 mass ppm or less, 5000 mass ppm or less, or 4000 mass ppm or less. In addition, in one embodiment, the amount of chlorine atoms bonded in the aromatic polyether (Cl-1) is 10 to 10000 mass ppm, 500 to 6000 mass ppm, 1000 to 5000 mass ppm, or 2000 to 4000 mass ppm. In addition, in one embodiment, the amount of chlorine atoms bonded in the aromatic polyether (Cl-1) may be 3000 to 5000 mass ppm.
[0096] In one embodiment, the content of inorganic chlorine (Cl-2) in the aromatic polyether is 0 mass ppm, 0 mass ppm or more, 10 mass ppm or more, 20 mass ppm or more, 35 mass ppm or more, or 50 mass ppm or more, and is 200 mass ppm or less, 100 mass ppm or less, 85 mass ppm or less, or 70 mass ppm or less. In addition, in one embodiment, the content of inorganic chlorine (Cl-2) in the aromatic polyether is 0 to 200 mass ppm, 10 to 100 mass ppm, 20 to 85 mass ppm, or 35 to 70 mass ppm.
[0097] In one embodiment, the total chlorine content (Cl-3) in the aromatic polyether is 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 500 mass ppm or more, 1000 mass ppm or more, or 2000 mass ppm or more, and is 10000 mass ppm or less, 6000 mass ppm or less, 5000 mass ppm or less, or 4000 mass ppm or less. In addition, in one embodiment, the total chlorine content (Cl-3) in the aromatic polyether is 10 to 10000 mass ppm, 100 to 10000 mass ppm, 500 to 6000 mass ppm, 1000 to 5000 mass ppm, or 2000 to 4000 mass ppm. In addition, in one embodiment, the total chlorine content (Cl-3) in the aromatic polyether may be 3000 to 5000 mass ppm.
[0098] A fluorine atom may or may not be bonded to the aromatic polyether.
[0099] In one embodiment, the amount of fluorine atoms bonded in the aromatic polyether (F-1) is 0 mass ppm, 0 mass ppm or more, 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 300 mass ppm or more, 500 mass ppm or more, or 1000 mass ppm or more, and is 10000 mass ppm or less, 5000 mass ppm or less, 2500 mass ppm or less, 2000 mass ppm or less, 1500 mass ppm or less, or 1200 mass ppm or less. In addition, in one embodiment, the amount of fluorine atoms bonded in the aromatic polyether (F-1) is 0 to 10000 mass ppm, 10 to 10000 mass ppm, 100 to 5000 mass ppm, 300 to 2500 mass ppm, 500 to 2000 mass ppm, 500 to 1500 mass ppm, or 500 to 1200 mass ppm. Furthermore, in one embodiment, the amount of fluorine atoms bonded to the aromatic polyether (F-1) may be 300 to 1000 mass ppm.
[0100] In one embodiment, the content of inorganic fluorine in the aromatic polyether (F-2) is 0 mass ppm, 0 mass ppm or more, 10 mass ppm or more, 20 mass ppm or more, 30 mass ppm or more, or 50 mass ppm or more, and is 200 mass ppm or less, 100 mass ppm or less, 90 mass ppm or less, or 85 mass ppm or less. In addition, in one embodiment, the content of inorganic fluorine in the aromatic polyether (F-2) is 0 to 200 mass ppm, 20 to 200 mass ppm, 30 to 100 mass ppm, 50 to 100 mass ppm, or 50 to 90 mass ppm.
[0101] In one embodiment, the total fluorine content (F-3) in the aromatic polyether is 0 mass ppm, 0 mass ppm or more, 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 300 mass ppm or more, 500 mass ppm or more, or 1000 mass ppm or more, and is 10000 mass ppm or less, 5000 mass ppm or less, 2500 mass ppm or less, 2000 mass ppm or less, 1500 mass ppm or less, or 1200 mass ppm or less. In addition, in one embodiment, the total fluorine content (F-3) in the aromatic polyether is 10 to 10000 mass ppm, 50 to 5000 mass ppm, 100 to 2500 mass ppm, 100 to 2000 mass ppm, 300 to 2000 mass ppm, 300 to 1500 mass ppm, 500 to 1500 mass ppm, or 500 to 1200 mass ppm. Furthermore, in one embodiment, the total fluorine content (F-3) in the aromatic polyether may be 300 to 1000 ppm by mass.
[0102] In one embodiment, the amount of potassium atoms contained as free components in the aromatic polyether is 20 mass ppm or more, 30 mass ppm or more, or 50 mass ppm or more, and is 150 mass ppm or less, 100 mass ppm or less, or 80 mass ppm or less. In addition, in one embodiment, the amount of potassium atoms contained as free components in the aromatic polyether is 20 to 150 mass ppm, 30 to 100 mass ppm, or 30 to 80 mass ppm.
[0103] In one embodiment, the amount of sodium atoms contained as free components in the aromatic polyether is 20 mass ppm or more, 30 mass ppm or more, or 50 mass ppm or more, and is 150 mass ppm or less, 100 mass ppm or less, or 90 mass ppm or less. In addition, in one embodiment, the amount of sodium atoms contained as free components in the aromatic polyether is 20 to 150 mass ppm, 30 to 100 mass ppm, or 50 to 90 mass ppm.
[0104] The aromatic polyether may contain an aromatic polyether to which a chlorine atom is bonded (hereinafter, sometimes referred to as component (a-1)) and an aromatic polyether to which a fluorine atom is bonded (hereinafter, sometimes referred to as component (a-2)).
[0105] The amount of chlorine atoms bonded in the component (a-1) is, for example, 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 500 mass ppm or more, 1000 mass ppm or more, or 2000 mass ppm or more, and is 10000 mass ppm or less, 6000 mass ppm or less, 5000 mass ppm or less, or 4000 mass ppm or less. In addition, the amount of chlorine atoms bonded in the component (a-1) is, for example, 10 to 10000 mass ppm, 500 to 6000 mass ppm, 1000 to 5000 mass ppm, or 2000 to 4000 mass ppm. In addition, in one embodiment, the amount of chlorine atoms bonded in the component (a-1) may be 3000 to 5000 mass ppm.
[0106] The amount of fluorine atoms bonded in the component (a-2) is, for example, 0 mass ppm, 0 mass ppm or more, 10 mass ppm or more, 50 mass ppm or more, 100 mass ppm or more, 300 mass ppm or more, 500 mass ppm or more, or 1000 mass ppm or less, 10000 mass ppm or less, 5000 mass ppm or less, 2500 mass ppm or less, 2000 mass ppm or less, 1500 mass ppm or less, or 1200 mass ppm or less. The amount of fluorine atoms bonded in the component (a-2) is, for example, 0 to 10000 mass ppm, 10 to 10000 mass ppm, 50 to 5000 mass ppm, 100 to 2500 mass ppm, 100 to 2000 mass ppm, 300 to 2000 mass ppm, 300 to 1500 mass ppm, 500 to 1500 mass ppm, or 500 to 1200 mass ppm. Furthermore, in one embodiment, the amount of fluorine atoms bonded to the component (a-2) may be 300 to 1000 mass ppm.
[0107] In one embodiment, the mass ratio of component (a-1) to component (a-2) is preferably 1:99 to 100:0, 1:99 to 99:1, 21:79 to 99:1, 25:75 to 95:5, 30:70 to 90:10, and more preferably 40:60 to 80:20. In another embodiment, the mass ratio of component (a-1) to component (a-2) is preferably 50:50 to 80:20.
[0108] In one embodiment, the composition includes, as the aromatic polyether, an aromatic polyether formed using 4,4'-dichlorobenzophenone as a monomer component.
[0109] In one embodiment, the composition contains, as aromatic polyethers, an aromatic polyether formed from 4,4'-dichlorobenzophenone as a monomer component (hereinafter sometimes referred to as component (a-1')) and an aromatic polyether formed from 4,4'-difluorobenzophenone as a monomer component (hereinafter sometimes referred to as component (a-2')).
[0110] The mass ratio of the component (a-1') to the component (a-2') is preferably 1:99 to 100:0, 1:99 to 99:1, 21:79 to 99:1, 25:75 to 95:5, 30:70 to 90:10, and more preferably 40:60 to 80:20. In one embodiment, the mass ratio of the component (a-1') to the component (a-2') is preferably 50:50 to 80:20.
[0111] In one embodiment, the structural unit represented by formula (1) is disposed at one or more ends of the main chain of the aromatic polyether. In this case, the terminal structure bonded to the structural unit may be a halogen atom. The halogen atom may be, for example, a chlorine atom (Cl) or a fluorine atom (F).
[0112] In one embodiment, a structural unit represented by formula (2) is arranged at one or more ends of the main chain of the aromatic polyether. In this case, the terminal structure bonded to the structural unit may be, for example, a hydrogen atom (H) or the like (when the terminal structure is a hydrogen atom (H), it forms a hydroxyl group together with the oxygen atom (O) in the structural unit.).
[0113] The terminal structure of the aromatic polyether may be, for example, a structure in which the above-mentioned chlorine atom (Cl) or hydroxyl group is replaced by a hydrogen atom (H). In addition, the terminal structure may have a structure other than the above-exemplified structures.
[0114] In one embodiment, the aromatic polyether includes a repeating unit represented by the following formula (3).
[0115]
Chemical formula 7
[0116]
[0117] The structural unit represented by formula (3) is a combination of the structural unit represented by formula (1) and the structural unit represented by formula (2).
[0118] In one embodiment, the aromatic polyether does not contain any other structure other than the structural units represented by formula (1) and formula (2).
[0119] In one embodiment, the aromatic polyether contains other structures other than the structural units represented by formula (1) and formula (2) within a range not impairing the effects of the present invention.
[0120] In one embodiment, based on all the monomers provided for the reaction, the total ratio (mass %) of the structural unit represented by formula (1) and the structural unit represented by formula (2) contained in all the monomers is 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, 90 mass % or more, 95 mass % or more, 97 mass % or more, 99 mass % or more, 99.5 mass % or more, and is 100 mass % or less, 99.9 mass % or less, or 100 mass %.
[0121] In one embodiment, in the aromatic polyether, the molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) (structural unit represented by formula (1):structural unit represented by formula (2)) is 47.5:52.5-52.5:47.5, 48.0:52.0-52.0:48.0, 48.5:51.5-51.5:48.5, 49.0:51.0-51.0:49.0 or 49.5:50.5-50.5:49.5.
[0122] The mol number of the structural unit represented by formula (1) may be greater than the mol number of the structural unit represented by formula (2), may be less than the mol number of the structural unit represented by formula (2), or may be the same as the mol number of the structural unit represented by formula (2).
[0123] In one embodiment, with respect to the aromatic polyether, 1 In H-NMR measurement, the α position of the hydroxyl group is assigned to 1 The peak of H relative to the main chain belongs to 1 The area ratio of the peak of H (hereinafter, sometimes referred to as "area ratio X") is less than 0.1%.
[0124] It should be noted that the area ratio X is recorded in the examples. 1 The value obtained by H-NMR measurement.
[0125] In one embodiment, the aromatic polyether is composed of one type of aromatic polyether having the same area ratio X.
[0126] In one embodiment, the aromatic polyether of the present embodiment is a mixture of two or more aromatic polyethers having different area ratios X. In this case, 1 In H-NMR measurement, the above-mentioned area ratio X can be achieved. Here, the above-mentioned two or more aromatic polyethers may or may not contain an aromatic polyether having an area ratio X of 0.1% or more.
[0127] The area ratio X of the aromatic polyether with an area ratio X of 0.1% or more may be, for example, 0.12% or more or 0.14% or more, or may be 2.0% or less, 1.8% or less, or 1.6% or less. In addition, the area ratio X of the aromatic polyether with an area ratio X of 0.1% or more may be, for example, 0.10 to 2.0%, 0.12 to 1.8%, or 0.14 to 1.6%.
[0128] In one embodiment, when 4,4'-dichlorobenzophenone and hydroquinone are used to synthesize an aromatic polyether, the area ratio X can be made less than 0.1% by making the molar ratio of 4,4'-dichlorobenzophenone to hydroquinone greater than 1.00.
[0129] In one embodiment, when 4,4'-difluorobenzophenone and hydroquinone are used to synthesize an aromatic polyether, the area ratio X can be made less than 0.1% by making the molar ratio of 4,4'-difluorobenzophenone to hydroquinone greater than 1.00.
[0130] The method for producing the aromatic polyether is not particularly limited.
[0131] In one embodiment, the method for producing an aromatic polyether includes the step of producing the (a-1′) component.
[0132] In one embodiment, a method of making an aromatic polyether comprises:
[0133] A step of manufacturing component (a-1');
[0134] a step of manufacturing component (a-2'); and
[0135] A step of mixing the component (a-1') and the component (a-2').
[0136] The method for producing the component (a-1') is not particularly limited.
[0137] In one embodiment, the method for producing the component (a-1′) includes the step of reacting 4,4′-dichlorobenzophenone with hydroquinone.
[0138] 4,4'-Dichlorobenzophenone and hydroquinone are monomers used for polymerizing the component (a-1').
[0139] Through the step of reacting 4,4'-dichlorobenzophenone and hydroquinone, (a-1') can be obtained as a copolymer of these compounds (monomer units).
[0140] 4,4'-Dichlorobenzophenone and hydroquinone are also commercially available.
[0141] In the following description, "reaction mixture" refers to the reaction system from the reaction of 4,4'-dichlorobenzophenone and hydroquinone to the end of the reaction, preferably in the form of a solution containing a solvent described later in addition to these monomers. The composition of the reaction mixture may change as the reaction proceeds. Usually, as the reaction proceeds, the concentration of the reactants (4,4'-dichlorobenzophenone and hydroquinone) in the reaction mixture decreases, and the concentration of the product ((a-1') component) increases.
[0142] The “maximum temperature” of the reaction mixture refers to the highest temperature (maximum achieved temperature) reached by the reaction mixture in the process from the start to the end of the reaction of 4,4′-dichlorobenzophenone and hydroquinone.
[0143] In one embodiment, the maximum temperature of the reaction mixture may be 260°C or more, 265°C or more, 270°C or more, 275°C or more, 280°C or more, 285°C or more, 290°C or more, more than 290°C, 295°C or more, 300°C or more, 305°C or more, 310°C or more, 315°C or more, 320°C or more, 325°C or more, 330°C or more, or 335°C or more. The upper limit is not particularly limited, and is, for example, 360°C or less. In addition, the maximum temperature of the reaction mixture is, for example, 260 to 360°C, preferably more than 290°C and 360°C or less, and more preferably 295 to 360°C.
[0144] In one embodiment, the method for producing component (a-1') comprises heating the reaction mixture to 150° C. or higher and then maintaining the temperature. The temperature during the temperature maintenance is not particularly limited, and may be, for example, 150 to 360° C. The temperature maintenance time is not particularly limited, and may be, for example, 0.1 to 12 hours.
[0145] In one embodiment, the method for producing component (a-1') comprises heating the reaction mixture to 150°C or higher, and then heating and maintaining the temperature once, or comprises repeating heating and maintaining the temperature a plurality of times. The number of repetitions is not particularly limited, and may be, for example, 2, 3, 4, 5, 6, 7, 8, 9 or 10 times.
[0146] By repeating the temperature increase and temperature maintenance multiple times, the reaction can be efficiently carried out.
[0147] In one embodiment, the method for producing the component (a-1') includes the step of maintaining the reaction mixture at 180 to 220°C for 0.5 to 2 hours, preferably 0.6 to 1.8 hours, and more preferably 0.7 to 1.5 hours (hereinafter also referred to as "temperature maintenance (i)"). This can promote the reaction while suppressing the volatilization of the raw materials, and can obtain a component (a-1') with a higher molecular weight.
[0148] In one embodiment, the method for producing the component (a-1') includes the step of maintaining the reaction mixture at 230 to 270°C for 0.5 to 2 hours, preferably 0.6 to 1.8 hours, and more preferably 0.7 to 1.5 hours (hereinafter also referred to as "temperature maintenance (ii)"). This can promote the reaction while suppressing the volatilization of the raw materials, and can obtain a component (a-1') with a higher molecular weight.
[0149] In one embodiment, the method for producing the component (a-1') includes the step of maintaining the reaction mixture at 280 to 360°C for 1 to 8 hours, preferably 1 to 6 hours, more preferably 1 to 4 hours (hereinafter also referred to as "temperature maintenance (iii)"). In this way, the component (a-1') having a desired molecular weight can be obtained.
[0150] In one embodiment, the method for producing component (a-1') may include two or three of the temperature maintenance steps (i) to (iii). The two or three temperature maintenance steps are preferably performed sequentially starting from the lower temperature. The two or three temperature maintenance steps may include a step of heating the reaction mixture.
[0151] The heating rate when heating the reaction mixture is not particularly limited, and may be, for example, 0.1 to 15°C / min, 0.1 to 10°C / min, 0.1 to 8°C / min, or 0.1 to 5°C / min. This can promote the reaction while suppressing volatilization of the raw materials, and can obtain a higher molecular weight component (a-1').
[0152] In one embodiment, in the method for producing the component (a-1′), the time from when the temperature of the reaction mixture reaches 150° C. to when the temperature reaches the maximum temperature is 2.0 to 10 hours.
[0153] In one embodiment, the reaction mixture comprises a solvent. The reaction mixture comprising a solvent may be in the form of a solution. The solution may comprise 4,4'-dichlorobenzophenone and hydroquinone dissolved in the solvent.
[0154] The solvent is not particularly limited, and for example, a neutral polar solvent can be used. Examples of the neutral polar solvent include N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dipropylacetamide, N,N-dimethylbenzoic acid amide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-isobutyl-2-pyrrolidone, N-n-propyl-2-pyrrolidone, N-n-butyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N-methyl-3-methyl -2-pyrrolidone, N-ethyl-3-methyl-2-pyrrolidone, N-methyl-3,4,5-trimethyl-2-pyrrolidone, N-methyl-2-piperidone, N-ethyl-2-piperidone, N-isopropyl-2-piperidone, N-methyl-6-methyl-2-piperidone, N-methyl-3-ethylpiperidone, dimethyl sulfoxide, diethyl sulfoxide, 1-methyl-1-oxocyclopentane, 1-ethyl-1-oxocyclopentane, 1-phenyl-1-oxocyclopentane, N,N'-dimethylimidazolidinone, diphenyl sulfone, etc.
[0155] In one embodiment, the reaction mixture contains aromatic sulfone, and the content of the solvent having a boiling point of 270 to 330° C. is 0 to less than 1 part by mass based on 100 parts by mass of the aromatic sulfone. This makes it easy to control the reaction temperature.
[0156] The reaction mixture may contain one or more solvents. It is particularly preferred that the reaction mixture contains only one solvent (single solvent) as a solvent, thereby simplifying the process.
[0157] In one embodiment, the reaction mixture comprises a base. By including a base in the reaction mixture, the reaction is facilitated.
[0158] The base is not particularly limited, and for example, an alkali metal salt is preferred. The alkali metal salt is not particularly limited, and examples thereof include alkali metal carbonates, alkali metal hydrogen carbonates, alkali metal hydride salts, and alkali metal hydroxides.
[0159] Examples of the alkali metal carbonate include potassium carbonate, sodium carbonate, lithium carbonate, rubidium carbonate, and cesium carbonate.
[0160] Examples of the alkali metal hydrogen carbonate include lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, rubidium hydrogen carbonate, and cesium hydrogen carbonate.
[0161] Among them, potassium carbonate is particularly preferred.
[0162] These bases may be used alone or in combination of two or more.
[0163] In one embodiment, the reaction mixture comprises potassium carbonate.
[0164] In one embodiment, the reaction mixture comprises other bases besides potassium carbonate. These bases can be used in combination with potassium carbonate. For example, potassium carbonate and sodium carbonate can also be used in combination.
[0165] The total concentration of the bases in the reaction mixture is not particularly limited.
[0166] In one embodiment, the total amount of alkali in the reaction mixture is 100 mol parts or more, and is 180 mol parts or less, 160 mol parts or less, 140 mol parts or less, or 120 mol parts or less, relative to 100 mol parts of hydroquinone added to the reaction mixture. If the total amount of alkali is 100 mol parts or more, the reaction time can be shortened. If the total amount of alkali is 180 mol parts or less, the formation of gel components can be suppressed. In addition, relative to 100 mol parts of hydroquinone added to the reaction mixture, the total amount of alkali in the reaction mixture is, for example, 100 to 180 mol parts, preferably 100 to 140 mol parts, and more preferably 100 to 120 mol parts.
[0167] In one embodiment, potassium carbonate is blended as the base in the above-mentioned blending amount.
[0168] The molar ratio ([DCBP]:[HQ]) of 4,4′-dichlorobenzophenone (DCBP) and hydroquinone (HQ) used in the reaction is not particularly limited.
[0169] The molar ratio ([DCBP]:[HQ]) can be appropriately adjusted for the purpose of controlling the molecular weight of the obtained component (a-1′).
[0170] In one embodiment, the molar ratio ([DCBP]:[HQ]) is 47.5:52.5-52.5:47.5, 48.0:52.0-52.0:48.0, 48.5:51.5-51.5:48.5, 49.0:51.0-51.0:49.0, or 49.5:50.5-50.5:49.5.
[0171] The mol number of 4,4'-dichlorobenzophenone (DCBP) may be greater than the mol number of hydroquinone (HQ), may be less than the mol number of hydroquinone (HQ), or may be the same as the mol number of hydroquinone (HQ).
[0172] In one embodiment, the total concentration of 4,4'-dichlorobenzophenone and hydroquinone in the reaction mixture (based on the amount of compounding) is not particularly limited, and is, for example, 1.0 mol / l or more, 1.2 mol / l or more, 1.3 mol / l or more, 1.4 mol / l or more, or 1.5 mol / l or more, and is 6.0 mol / l or less, 5.0 mol / l or less, or 4.0 mol / l or less. In addition, the total concentration of 4,4'-dichlorobenzophenone and hydroquinone in the reaction mixture (based on the amount of compounding) is, for example, 1.0 to 6.0 mol / l, preferably 1.3 to 5.0 mol / l, and more preferably 1.5 to 4.0 mol / l.
[0173] In one embodiment, as monomers provided for the above reaction, no monomers other than 4,4′-dichlorobenzophenone and hydroquinone are used.
[0174] In one embodiment, in the above reaction, other monomers other than 4,4′-dichlorobenzophenone and hydroquinone are used in combination within a range that does not impair the effects of the present invention.
[0175] In one embodiment, the total ratio (mass %) of 4,4'-dichlorobenzophenone and hydroquinone based on all monomers used in the reaction is 50 mass % or more, 60 mass % or more, 70 mass % or more, 80 mass % or more, 90 mass % or more, 95 mass % or more, 97 mass % or more, 99 mass % or more, 99.5 mass % or more, or 100 mass %.
[0176] In one embodiment, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 99% by mass or more, 99.5% by mass or more, 99.9% by mass or more, or substantially 100% by mass of the reaction mixture at the start of the reaction is:
[0177] 4,4'-dichlorobenzophenone, hydroquinone, alkali metal salt and solvent,
[0178] 4,4'-dichlorobenzophenone, hydroquinone, one or more alkali metal salts selected from potassium carbonate and sodium carbonate, and diphenyl sulfone, or
[0179] 4,4'-Dichlorobenzophenone, hydroquinone, potassium carbonate and diphenyl sulfone.
[0180] In addition, in the case of "substantially 100 mass %", unavoidable impurities may be contained.
[0181] The reaction of 4,4'-dichlorobenzophenone and hydroquinone can be carried out in an inert gas atmosphere. The inert gas is not particularly limited, and examples thereof include nitrogen and argon.
[0182] The method for producing the component (a-2') is not particularly limited.
[0183] In one embodiment, the method for producing the component (a-2′) includes the step of reacting 4,4′-difluorobenzophenone with hydroquinone.
[0184] The component (a-2′) can be produced in the same manner as the method for producing the component (a-1′) except that 4,4′-difluorobenzophenone is used instead of 4,4′-dichlorobenzophenone.
[0185] In one embodiment, the component (a-1′) is the component (a-1).
[0186] In one embodiment, the component (a-2′) is the component (a-2).
[0187] As the aromatic polyether, the component (a-1') may be used alone or as a mixture of the component (a-1') and the component (a-2'). When a mixture is used, the mixing ratio (mass ratio) of the component (a-1') and the component (a-2') may be adjusted to prepare an aromatic polyether having a bound chlorine atom content of 10 to 10,000 ppm.
[0188] The method for mixing the component (a-1') and the component (a-2') is not particularly limited, and examples thereof include mixing using a known mixer, melt kneading using an extruder, etc. Specifically, for example, the component (a-1') and the component (a-2') can be kneaded using a twin-screw kneader or the like in a state where the components are heated to 360°C to 440°C and melted. At this time, the component (a-1') and the component (a-2') can be kneaded to obtain an aromatic polyether, and then the non-continuous carbon fiber can be kneaded in the aromatic polyether, or the component (a-1'), the component (a-2') and the non-continuous carbon fiber can be kneaded together.
[0189] Regarding the mixing ratio of the components (a-1') and (a-2'), by increasing the proportion of the component (a-1'), the amount of chlorine atoms bonded to the aromatic polyether in the mixture (aromatic polyether) can be increased, and the amount of fluorine atoms bonded to the aromatic polyether can be reduced.
[0190] (Discontinuous carbon fiber)
[0191] In this specification, "non-continuous carbon fiber" refers to carbon fiber having an average fiber length of 20 mm or less.
[0192] In one embodiment, the non-continuous carbon fibers are chopped strands. Thus, the strength of the composition is further improved.
[0193] In one embodiment, the composition may be a fiber composite material comprising an aromatic polyether as a matrix and discontinuous carbon fibers as reinforcing fibers. The fiber composite material may be a so-called fiber reinforced thermoplastic (FRTP).
[0194] In one embodiment, the average fiber length of the discontinuous carbon fibers is 0.5 to 20 mm, 0.5 to 10 mm, 1 to 7 mm, or 2 to 6 mm. The average fiber length of the discontinuous carbon fibers is obtained from the arithmetic mean of values measured with a vernier caliper.
[0195] In one embodiment, the average fiber diameter of the discontinuous carbon fibers is 1 to 30 μm. From the viewpoint of the dispersibility of the discontinuous carbon fibers in the aromatic polyether, the surface smoothness and mechanical strength of the molded product, the average fiber diameter of the discontinuous carbon fibers is preferably 3 to 25 μm, 6 to 20 μm, and more preferably 6 to 13 μm. The average fiber diameter of the discontinuous carbon fibers is obtained by the arithmetic mean of the values measured in accordance with JIS R 7607:2000.
[0196] The non-continuous carbon fibers can be treated with a sizing agent. The non-continuous carbon fibers can be bundled into bundles by the sizing agent. The non-continuous carbon fibers treated with the sizing agent have the sizing agent attached to their surface. The sizing agent is not particularly limited, and examples thereof include epoxy sizing agents, urethane sizing agents, polyamide sizing agents, and the like. In addition, aromatic polyethers can also be used as sizing agents. As sizing agents, one of them can be used alone, or two or more can be used in combination. As non-continuous carbon fibers, non-continuous carbon fibers that have not been treated with a sizing agent can be used. Silane coupling agents such as aminosilane, isocyanate silane, and acrylic silane can be used in combination with the above-mentioned sizing agents.
[0197] The content of the non-continuous carbon fibers in the composition is not particularly limited.
[0198] In one embodiment, the content of the discontinuous carbon fiber is 5 parts by mass or more, 10 parts by mass or more, 20 parts by mass or more, 30 parts by mass or more, or 40 parts by mass or more, and is 100 parts by mass or less, 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, 60 parts by mass or less, 55 parts by mass or less, or 50 parts by mass or less. In addition, in one embodiment, the content of the discontinuous carbon fiber is 5 to 100 parts by mass, 5 to 80 parts by mass, 5 to 60 parts by mass, 10 to 60 parts by mass, 20 to 55 parts by mass, 30 to 50 parts by mass, or 40 to 50 parts by mass relative to 100 parts by mass of the aromatic polyether. By making the content of the discontinuous carbon fiber 5 parts by mass or more relative to 100 parts by mass of the aromatic polyether, the reinforcing effect brought by the discontinuous carbon fiber can be more suitably obtained. In addition, by being 100 parts by mass or less, and further being 60 parts by mass or less, the adaptability of the composition during mixing and molding is further improved.
[0199] The composition may include other components other than the aromatic polyether and the discontinuous carbon fiber. The other components are not particularly limited, and for example, other resins other than the aromatic polyether may be cited. As other resins, for example, fluororesins such as polytetrafluoroethylene may be cited. As other components, one may be used alone, or two or more may be used in combination.
[0200] In one embodiment, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, and 100% by mass or less, 99.9% by mass or less, or substantially 100% by mass of the composition is:
[0201] Aromatic polyether and discontinuous carbon fiber,
[0202] Aromatic polyether, discontinuous carbon fibers and the above other ingredients.
[0203] In addition, in the case of "substantially 100 mass %", unavoidable impurities may be contained.
[0204] The method for preparing the composition is not particularly limited, and examples thereof include mixing with a known mixer, melt kneading with an extruder, etc. The discontinuous carbon fibers may be side-fed to the aromatic polyether using a twin-screw kneader.
[0205] The composition can be pelletized and used as a raw material for producing a shaped body.
[0206] In one embodiment, the method for producing pellets includes the steps of chopping discontinuous carbon fibers into chopped strands and then adding an aromatic polyether to the discontinuous carbon fibers. Pellets (also referred to as "short fiber pellets") can be produced by mixing short fibers and aromatic polyethers and pelletizing them.
[0207] In one embodiment, the pellet manufacturing method is to immerse the roving of the discontinuous carbon fiber in a molten aromatic polyether and perform pultrusion, and then cut it into a desired pellet length to manufacture the pellet (also referred to as "long fiber pellet"). When the long fiber pellet is manufactured as described above, the breakage of the discontinuous carbon fiber can be suppressed.
[0208] By shaping the composition (which may be in the form of the above-mentioned pellets), a molded body can be manufactured. The molding can be performed using known methods such as injection molding, extrusion molding, and blow molding. In addition, the composition can also be stamped, and known methods such as cold pressing and hot pressing can be used. In addition, the composition can also be used as a resin composition for a 3D printer and molded using a 3D printer.
[0209] In one embodiment, the composition has a tensile strength of 2.80 times or more, more than 2.87 times, more than 2.88 times, more than 2.90 times, more than 2.95 times, or more than 3.00 times relative to the tensile strength of the aromatic polyether alone. The upper limit of this ratio (also referred to as "increase rate") is not particularly limited, for example, 5.00 times or less or 4.00 times or less. In addition, in one embodiment, the composition has a tensile strength of 2.80 to 5.00 times, 2.88 to 5.00 times, or 2.95 to 4.00 times relative to the tensile strength of the aromatic polyether alone. In addition, in one embodiment, the composition has a tensile strength of 2.35 to 5.00 times, 2.45 to 4.00 times, 2.50 to 3.00 times, or 2.50 to 2.75 times relative to the tensile strength of the aromatic polyether alone.
[0210] In addition, the tensile strength of the composition and the tensile strength of the aromatic polyether alone were measured by the following method.
[0211] The composition (or the aromatic polyether alone) was injection molded at 400° C. using a small molding machine (MiniJet-Pro manufactured by Haake) to produce a dumbbell-shaped 5A type specified in ISO 527-2:2012 as a test piece.
[0212] The obtained test piece was subjected to a tensile test at a test speed of 5 mm / min and a distance between clamps of 50 mm to measure the tensile strength.
[0213] It should be noted that, as preparation for the tensile test, the upper and lower clamps of the tensile tester were aligned to the position of the predetermined distance between the clamps (50 mm), the test piece was held by the lower clamp, and the load zero point adjustment was performed. Then, the test piece was held by the upper clamp, and the tensile test was started.
[0214] In one embodiment, the tensile strength of the composition is 270 MPa or more, 280 MPa or more, 290 MPa or more, 300 MPa or more, 310 MPa or more, 320 MPa or more, 350 MPa or less, or 330 MPa or more. The upper limit is not particularly limited, for example, 500 MPa or less or 400 MPa or less. In addition, in one embodiment, the tensile strength of the composition is 270 to 500 MPa, 290 to 400 MPa, or 300 to 350 MPa. In addition, in one embodiment, the tensile strength of the composition is 230.0 to 400.0 MPa, 235.0 to 350.0 MPa, 240.0 to 300.0 MPa, or 250.0 to 300.0 MPa.
[0215] The use of the composition of the present invention is not particularly limited, and can be widely used in various applications requiring strength. The composition of the present invention is particularly suitable for applications requiring heat resistance, solvent resistance, and durability, for example, as a metal replacement material. More specifically, it is suitable for bearings, gaskets, structural materials, etc.
[0216] The composition of the second embodiment of the present invention comprises an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by formula (1) and a structural unit represented by formula (2), and the total chlorine content (Cl-3) in the aromatic polyether is 10 to 10000 mass ppm.
[0217] According to the second aspect, the same effects as those of the first aspect can be obtained.
[0218] The composition of the third embodiment of the present invention comprises an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by formula (1) and a structural unit represented by formula (2), and the ratio of the total chlorine content (Cl-3) in the aromatic polyether to the total chlorine content (Cl-3) in the aromatic polyether and the total fluorine content (F-3) in the aromatic polyether (also referred to as "ratio (Cl / (Cl+F))") is 40 to 100% by mass.
[0219] According to the third aspect, the same effects as those of the first aspect can be obtained.
[0220] In the third aspect, the ratio (Cl / (Cl+F)) is preferably 40 to 100 mass %, 50 to 95 mass %, and more preferably 60 to 85 mass %. In one embodiment, the ratio (Cl / (Cl+F)) is preferably 70 to 85 mass %.
[0221] In the second and third embodiments, it is preferred that the total chlorine content (Cl-3) in the aromatic polyether is 100 to 10,000 ppm by mass, and the total fluorine content (F-3) in the aromatic polyether is 100 to 2,000 ppm by mass. Thus, the effect of the present invention is better exerted. It should be noted that the total chlorine content (Cl-3) in the aromatic polyether and the total fluorine content (F-3) in the aromatic polyether are not limited to the ranges exemplified herein, and the ranges exemplified for the composition of the first embodiment can be appropriately applied.
[0222] Regarding the compositions of the second and third embodiments, the description of the compositions of the first embodiment is cited. Among them, the compositions of the second and third embodiments are not limited to the compositions of the first embodiment (i.e., compositions comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by formula (1) and a structural unit represented by formula (2), and the amount of chlorine atoms bonded in the aromatic polyether is 10 to 10,000 ppm). It should be noted that the composition of the present invention may satisfy any two or more of the conditions of the first, second and third embodiments. For example, there may be cited compositions that simultaneously satisfy the conditions of the first and second embodiments, compositions that simultaneously satisfy the conditions of the first and third embodiments, compositions that simultaneously satisfy the conditions of the second and third embodiments, and compositions that simultaneously satisfy the conditions of the first, second and third embodiments.
[0223] Example
[0224] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0225] 1. Preparation of Aromatic Polyether
[0226] Aromatic polyether (A-1)
[0227] In a 300 ml four-necked flask equipped with a stirrer, a thermometer, a nitrogen inlet tube, and a water recovery container connected to a condenser, 41.220 g (0.164 mol) of 4,4'-dichlorobenzophenone, 17.809 g (0.162 mol) of hydroquinone, 25.704 g (0.186 mol) of potassium carbonate, and 140.01 g of diphenyl sulfone were added, and nitrogen gas was allowed to flow.
[0228] The reaction mixture was reacted under the temperature control described below.
[0229] <Temperature Control>
[0230] (1) After heating to 150°C, heat to 200°C over 30 minutes
[0231] (2) Maintain at 200°C for 1 hour
[0232] (3) Heating from 200°C to 250°C (heating rate 1.7°C / min)
[0233] (4) Maintain at 250°C for 1 hour
[0234] (5) Heating from 250°C to 300°C (maximum temperature of the reaction mixture) (heating rate 3.0°C / min)
[0235] (6) Maintain at 300°C (maximum temperature of the reaction mixture) for 2 hours
[0236] After the reaction was completed, the product was pulverized with a stirrer (7010HS manufactured by Warling), washed with acetone and water in that order, and then dried in a dryer at 180° C. to obtain a powdery aromatic polyether.
[0237] The obtained aromatic polyether was used as aromatic polyether (A-1).
[0238] Aromatic polyether (A-2)
[0239] As the aromatic polyether (A-2), a commercially available aromatic polyether (151G manufactured by Victrex Corporation) was used.
[0240] 2. Preparation of the composition
[0241] (Example 1)
[0242] Using a twin-screw mixer (manufactured by Termo Fisher, Process 11), aromatic polyether (A-1), aromatic polyether (A-2) and discontinuous carbon fiber (manufactured by Mitsubishi Chemical, carbon fiber chopped fiber TR06U B4E, average fiber diameter 7 μm, average fiber length 6 mm) were mixed at a mass ratio of (A-1: A-2: discontinuous carbon fiber) 20:80:43 at 400°C to obtain a composition containing aromatic polyether (A-1), (A-2) and discontinuous carbon fiber.
[0243] 3. Determination method
[0244] (1) Tensile strength
[0245] The obtained composition was injection molded at 400°C using a small molding machine (MiniJet-Pro manufactured by Haake) to produce a dumbbell-shaped 5A type specified in ISO 527-2:2012 as a test piece.
[0246] The obtained test piece was subjected to a tensile test at a test speed of 5 mm / min and a distance between chucks of 50 mm to measure the tensile strength (also referred to as "tensile strength of reinforced product").
[0247] It should be noted that, as preparation for the tensile test, the upper and lower clamps of the tensile tester were aligned to the position of the predetermined distance between the clamps (50 mm), the test piece was held by the lower clamp, and the load zero point adjustment was performed. Then, the test piece was held by the upper clamp, and the tensile test was started.
[0248] In addition, the tensile strength of the aromatic polyether (A) alone (pure product) without blending discontinuous carbon fibers was measured in the same manner as above (also referred to as “pure product tensile strength”).
[0249] Furthermore, the increase rate of the tensile strength of the reinforced product relative to the tensile strength of the pure product (also referred to as "reinforced product / pure product increase rate") was calculated.
[0250] (2) Determination of the amount of chlorine atoms and fluorine atoms bonded in aromatic polyethers The amount of chlorine atoms bonded in aromatic polyethers (Cl-1), the amount of chlorine atoms contained as free components in the aromatic polyethers (Cl-2, also referred to as "inorganic chlorine content"), and the total amount of these chlorine atoms (Cl-3, also referred to as "total chlorine content in aromatic polyethers") were determined by the following method. In addition, the amount of fluorine atoms bonded in aromatic polyethers (F-1), the amount of fluorine atoms contained as free components in the aromatic polyethers (F-2, also referred to as "inorganic fluorine content"), and the total amount of these fluorine atoms (F-3, also referred to as "total fluorine content in aromatic polyethers") were determined. In addition, the amount of potassium atoms and the amount of sodium atoms contained as free components in the aromatic polyethers were determined.
[0251] <Calculation of the Amount of Chlorine Atoms Bonded in Aromatic Polyether (Cl-1)>
[0252] a. The total chlorine content (mass ppm) (Cl-3) was calculated from the result of measuring the total chlorine amount (*1: described later) of the aromatic polyether.
[0253] b. For aromatic polyethers, the potassium content (mass ppm) is calculated from the measured value of the potassium amount (*2: described later), and the inorganic chlorine content (mass ppm) (Cl-2) is calculated by assuming that the inorganic chlorine (chlorine atoms not bonded to the aromatic polyether) is contained in an amount equimolar to potassium.
[0254] c. The amount of chlorine atoms bonded to the aromatic polyether (mass ppm) (Cl-1) was calculated by subtracting the content of inorganic chlorine (mass ppm) (Cl-2) from the content of total chlorine (mass ppm) (Cl-3).
[0255] <Calculation of the Amount of Fluorine Atoms Bonded to Aromatic Polyether (F-1)>
[0256] a. The total fluorine content (mass ppm) was calculated from the result of measuring the total fluorine content (*1: described later) of the aromatic polyether (F-3).
[0257] b. For the aromatic polyether, the sodium content (mass ppm) is calculated from the measured value of the sodium amount (*2: described later), and the inorganic fluorine content (mass ppm) is calculated (F-2) assuming that the inorganic fluorine (fluorine atoms not bonded to the aromatic polyether) is contained in an amount equal in mole to that of sodium.
[0258] c. The amount of fluorine atoms bonded to the aromatic polyether (mass ppm) (F-1) was calculated by subtracting the content of inorganic fluorine (mass ppm) (F-2) from the content of total fluorine (mass ppm) (F-3).
[0259] (*1) Determination method of total chlorine (Cl-3) and total fluorine (F-3) in aromatic polyethers
[0260] The sample (aromatic polyether) is introduced into a combustion furnace and burned in a combustion gas containing oxygen. After the generated gas is captured in an absorbent, the absorbent is separated and quantified using an ion chromatograph. The quantitative value is obtained based on a standard curve prepared based on a reference of known concentration. The measurement conditions are shown below.
[0261] <Sample Combustion>
[0262] Combustion device: AQF-2100H manufactured by Nittoseiko Analytech Co., Ltd.
[0263] Combustion furnace set temperature: front section 800, rear section 1100℃
[0264] Argon flow rate: 400ml / min
[0265] Oxygen flow rate: 200ml / min
[0266] Absorbent: Hydrogen peroxide
[0267] <Ion Chromatography>
[0268] Analytical device: Integrion manufactured by Thermo Fisher Scientific Co., Ltd.
[0269] Column: A guard column (Dionex IonPac AG12A) and a separation column (Dionex IonPac AS12A) were connected and used (both columns were manufactured by Thermo Fisher Scientific)
[0270] Eluent: Na2CO3 (2.7mmol / 1) + NaHCO3 (0.3mmol / 1)
[0271] Flow rate: 1.5ml / min
[0272] Column temperature: 30°C
[0273] Measurement mode: Suppression mode
[0274] Detector: Conductivity detector
[0275] (*2) Method for measuring the amount of potassium and sodium in aromatic polyethers (the amount of potassium atoms and the amount of sodium atoms contained as free components in aromatic polyethers)
[0276] The contents of potassium atoms (K) and sodium atoms (Na) in the aromatic polyether were determined by ICP emission spectrometry. The aromatic polyether was pretreated according to the following steps. Na was measured at 589.592 nm, and K was measured at 766.481 nm.
[0277] 1 g of a sample was weighed in a platinum dish, concentrated sulfuric acid was added thereto, and then heated to perform a carbonization treatment. Then, the platinum dish was placed in an electric furnace and ashing treatment was performed at 550° C. for 12 hours.
[0278] After the ashing treatment, hydrochloric acid is added, and then the mixture is heated. After cooling, the mixture is fixed to volume with ultrapure water. It should be noted that, in the case where the sample contains an inorganic filler (non-continuous carbon fiber), after the ashing treatment, hydrofluoric acid is added, and then the mixture is heated to dry solid. After cooling, hydrochloric acid is added, and then the mixture is heated. After cooling, the mixture is fixed to volume with ultrapure water.
[0279] The quantitative value is obtained based on a standard curve prepared from a reference of known concentration. The hydrochloric acid concentration of the standard curve solution is the same as that of the sample solution.
[0280] In addition, regarding the above-mentioned measured values, "-" in Table 1 means 6 mass ppm or less.
[0281] (Supplementary test)
[0282] Considering the possibility that 4,4'-difluorobenzophenone and 4,4'-dichlorobenzophenone, which are monomers (reactants) used in the synthesis, remain in the aromatic polyether, the amount of fluorine atoms contained as 4,4'-difluorobenzophenone and the amount of chlorine atoms contained as 4,4'-dichlorobenzophenone in the aromatic polyether were quantified by the following method.
[0283] First, the solid sample (aromatic polyether) is crushed with a stirrer, washed with acetone and water in sequence, and dried with an explosion-proof dryer at 180°C. It should be noted that when the reaction mixture (product) immediately after the reaction to produce the aromatic polyether is used as a sample, after the reaction is completed, the product is cooled and solidified to prepare the above-mentioned solid sample. The stirrer used is not particularly limited, and Warling 7010HS is used here.
[0284] Next, about 1 g of the dried sample was weighed in an eggplant-shaped flask, 100 ml of cyclohexanone and a boiling stone were added thereto, and the mixture was heated under reflux for 1 hour using a mantle heater. After cooling to room temperature, the solid content was removed by filtration.
[0285] Next, the obtained solution is measured by gas chromatography, thereby calculating the amount (mass ppm) of 4,4'-difluorobenzophenone and the amount (mass ppm) of 4,4'-dichlorobenzophenone in the sample. Here, the amount (mass ppm) of 4,4'-difluorobenzophenone and the amount (mass ppm) of 4,4'-dichlorobenzophenone in the sample are obtained based on a standard curve prepared based on a reference with a known concentration. The measurement conditions of gas chromatography are shown below.
[0286] <Gas Chromatography Measurement Conditions>
[0287] Analytical device: Agilent Technologies 8890
[0288] GC column: Agilent Technologies DB-HeavyWAX (length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm)
[0289] Inlet temperature: 250℃
[0290] Oven temperature: 250℃ (constant)
[0291] Flow rate: 1ml / min
[0292] Injection volume: 1μl
[0293] Split ratio: 40:1
[0294] Detector: FID
[0295] Detector temperature: 250
[0296] The amount (mass ppm) of fluorine atoms contained as 4,4′-difluorobenzophenone and the amount (mass ppm) of chlorine atoms contained as 4,4′-dichlorobenzophenone in the aromatic polyether were converted by the following calculation formula.
[0297] The amount of fluorine atoms contained in the aromatic polyether as 4,4'-difluorobenzophenone (mass ppm) = the amount of 4,4'-difluorobenzophenone in the sample (mass ppm) ÷ 218.20 (molecular weight of 4,4'-difluorobenzophenone) × 19.00 (atomic weight of fluorine) × 2 The amount of chlorine atoms contained in the aromatic polyether as 4,4'-dichlorobenzophenone (mass ppm) = the amount of 4,4'-dichlorobenzophenone in the sample (mass ppm) ÷ 251.11 (4,4'-dichlorobenzophenone) As a result of the supplementary test of the above formula (molecular weight of ketone) × 35.45 (atomic weight of chlorine) × 2, the amount of fluorine atoms contained as 4,4'-difluorobenzophenone in the aromatic polyether (mass ppm) and the amount of chlorine atoms contained as 4,4'-dichlorobenzophenone (mass ppm) were both less than 100 mass ppm as the quantitative lower limit, so it was confirmed that there was no influence on the calculation results of the amount of fluorine atoms bonded in the aromatic polyether (F-1) and the amount of chlorine atoms bonded in the aromatic polyether (Cl-1).
[0298] In addition, based on the values of the total chlorine content (Cl-3) in the aromatic polyether and the total fluorine content (F-3) in the aromatic polyether, the ratio of the total chlorine content (Cl-3) in the aromatic polyether to the total of the total chlorine content (Cl-3) in the aromatic polyether and the total fluorine content (F-3) in the aromatic polyether is calculated ("ratio (Cl / (Cl+F))").
[0299] (3) 1 H-NMR measurement (area ratio X)
[0300] The aromatic polyether (A) used in the composition was subjected to 1H-NMR measurement according to the following procedure.
[0301] The aromatic polyether is provided 1 In H-NMR measurement, the ratio (area ratio X) of the peak area at the α position of the hydroxyl group (area with chemical shift from 6.98 ppm to 7.03 ppm) to the main chain peak area (area with chemical shift from 7.32 ppm to 7.36 ppm) was determined by the following formula.
[0302] Area ratio X[%] = (area of the peak at the α position of the hydroxyl group / area of the main chain peak) × 100
[0303] 1The measurement conditions of H-NMR measurement are as follows.
[0304] < 1 H-NMR measurement conditions>
[0305] ·NMR device: Ascend500 manufactured by Bruker Japan Co., Ltd.
[0306] Probe: 5mmφTCI low temperature probe
[0307] NMR sample tube diameter: 5mmφ
[0308] Preparation of sample solution: 0.6 ml of methanesulfonic acid was added to about 20 mg of a sample, and the mixture was stirred at room temperature for 1 hour. Then, 0.4 ml of deuterated dichloromethane was added, and the mixture was further stirred at room temperature for 30 minutes to dissolve the sample to prepare a sample solution.
[0309] Observation range: 20ppm
[0310] Observation center: 6.175ppm
[0311] Number of data points: 64kB
[0312] Pulse repetition time: 10 seconds
[0313] Total times: 256 times
[0314] Flip angle: 30°
[0315] ·Measurement temperature: 25℃
[0316] Chemical shift reference: The central peak among the three peaks of deuterated dichloromethane was set to 5.32 ppm
[0317] The above results are shown in Table 1.
[0318] (Example 2)
[0319] A composition was obtained in the same manner as in Example 1 except that the aromatic polyether (A) was used in a mass ratio of (A-1:A-2) of 40:60. The obtained composition was measured in the same manner as in Example 1. The results are shown in Table 1.
[0320] (Example 3)
[0321] A composition was obtained in the same manner as in Example 1 except that the aromatic polyether (A) was used in a mass ratio of (A-1:A-2) of 60:40. The obtained composition was measured in the same manner as in Example 1. The results are shown in Table 1.
[0322] (Example 4)
[0323] A composition was obtained in the same manner as in Example 1 except that the aromatic polyether (A) was used in a mass ratio (A-1:A-2) of 80:20. The obtained composition was measured in the same manner as in Example 1. The results are shown in Table 1.
[0324] (Example 5)
[0325] A composition was obtained in the same manner as in Example 1 except that the aromatic polyether (A) (A-1) and (A-2) were used at a mass ratio of (A-1:A-2) 100:0 (the aromatic polyether (A-2) was omitted). The obtained composition was measured in the same manner as in Example 1. The results are shown in Table 1.
[0326] (Comparative Example 1)
[0327] A composition was obtained in the same manner as in Example 1 except that the aromatic polyether (A) was used at a mass ratio (A-1:A-2) of 0:100 (the aromatic polyether (A-1) was omitted). The obtained composition was measured in the same manner as in Example 1. The results are shown in Table 1.
[0328]
Table 1
[0329] Several embodiments and / or examples of the present invention have been described in detail above, but those skilled in the art can easily make various changes to these illustrative embodiments and / or examples without departing from the novel teachings and effects of the present invention. Therefore, these various changes are included within the scope of the present invention.
[0330] The contents of the documents described in this specification and the applications serving as the basis for the Paris Convention priority claim of the present application are incorporated herein by reference in their entirety.
Claims
1. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), wherein the amount of chlorine atoms bonded to the aromatic polyether is 10 to 10,000 ppm by mass, 2. The composition according to claim 1, wherein The amount of fluorine atoms bonded to the aromatic polyether is 10 to 10000 mass ppm. 3 . The composition according to claim 1 , comprising an aromatic polyether formed using 4,4′-dichlorobenzophenone as a monomer component.
4. The composition according to any one of claims 1 to 3, wherein The aromatic polyether comprises a repeating unit represented by the following formula (3):
5. The composition according to any one of claims 1 to 4, wherein The average fiber length of the discontinuous carbon fibers is 0.5 mm to 20 mm.
6. The composition according to any one of claims 1 to 5, wherein The content of the discontinuous carbon fibers is 5 to 100 parts by mass based on 100 parts by mass of the aromatic polyether. 7 . The composition according to claim 1 , which has a tensile strength of 2.80 times or more the tensile strength of the aromatic polyether alone. 8 . The composition according to claim 1 , which has a tensile strength of 2.35 to 5.00 times the tensile strength of the aromatic polyether alone.
9. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), wherein the total chlorine content in the aromatic polyether is 10 to 10,000 ppm by mass, 10. A composition comprising an aromatic polyether and non-continuous carbon fibers, wherein the aromatic polyether comprises a structural unit represented by the following formula (1) and a structural unit represented by the following formula (2), wherein the ratio of the total chlorine content in the aromatic polyether to the total chlorine content in the aromatic polyether and the total fluorine content in the aromatic polyether is 40% by mass to 100% by mass, 11. The composition according to claim 9 or 10, wherein The total chlorine content in the aromatic polyether is 100 to 10000 mass ppm, and the total fluorine content in the aromatic polyether is 100 to 2000 mass ppm.
12. The composition according to any one of claims 9 to 11, wherein The aromatic polyether comprises a repeating unit represented by the following formula (3):
13. The composition according to any one of claims 9 to 12, wherein The average fiber length of the discontinuous carbon fibers is 0.5 mm to 20 mm.
14. The composition according to any one of claims 9 to 13, wherein The content of the discontinuous carbon fiber is 5 parts by mass to 100 parts by mass based on 100 parts by mass of the aromatic polyether. 15 . The composition according to claim 9 , which has a tensile strength of 2.80 times or more the tensile strength of the aromatic polyether alone. 16 . The composition according to claim 9 , which has a tensile strength of 2.35 to 5.00 times the tensile strength of the aromatic polyether alone.