Energy storage

By combining hydrated or hydratable inorganic salts with porous inorganic host materials to form composite thermochemical materials, the problems of stability and kinetic controllability of salt hydrates during thermal cycles are solved, and high energy density and mechanical properties are achieved. stability, improving the performance and efficiency of thermochemical energy storage.

CN118786197APending Publication Date: 2024-10-15WEITUO THERMAL TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380024539.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-03-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing thermochemical energy storage materials such as salt hydrates have stability and kinetic controllability issues during thermal cycling, resulting in a decrease in energy density and degradation of system performance, limiting their application in thermochemical processes.

Method used

Composite thermochemical materials containing hydrated or hydratable inorganic salts and porous inorganic host materials are used to form composite materials with high energy density and mechanical stability by mixing inorganic salts and porous host materials, using binders and flow aids Improve material properties.

Benefits of technology

Thermochemical materials with high energy density, mechanical stability and multiple cycles have been achieved, improving the heat and mass transfer rates of the materials, enhancing reaction kinetics, and reducing production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786197A_ABST
    Figure CN118786197A_ABST
Patent Text Reader

Abstract

A method of forming a composite thermochemical material, the method comprising providing an inorganic host material and providing a hydrated or hydratable inorganic salt, mixing the inorganic host material and the hydrated or hydratable inorganic salt to form a mixture, allowing or causing at least a portion of the hydrated or hydratable inorganic salt to enter the pores and / or void spaces of the inorganic host material, and forming the mixture into a shaped body.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates generally to energy storage. More particularly, but not exclusively, the present invention relates to thermochemical materials for thermal energy storage.

[0002] Global energy consumption is still dominated by fossil fuels. Environmental impacts associated with the use of fossil fuels, such as climate change, have become significant issues. There are multiple pathways to decarbonize the global energy system, and almost all of them rely on deep penetration of renewable generation, which requires energy storage to address the challenge of supply-demand mismatch.

[0003] Thermochemical energy storage (TCES) is one of the three thermal energy storage (TES) technologies used to address the mismatch between supply and demand. TES technology based on TCES is based on reversible thermochemical reactions and / or adsorption processes, where energy is stored in the form of chemical compounds produced by an endothermic process and recovered when needed by recombining the compounds in an exothermic process. The principle of such a technology can be simply illustrated by the following scheme:

[0004] Charging: C+heat → A+B

[0005] Storage: A and B are stored separately (no or almost no heat loss)

[0006] Discharging: A+B→C+heat

[0007] Wherein A, B and C are reactants or products depending on the charging or releasing process. Examples of A include hydroxides, hydrates, carbonates and ammonia compounds; and examples of B include water, CO, ammonia and hydrogen. C can be in solid or liquid form, and A and B can be in any phase. The heat stored in the TCES system is proportional to the amount of TCES material, the heat of reaction and / or adsorption, and the extent of the reaction / adsorption process. Since the chemical compounds produced during the charging process can be stored separately, there is no energy loss during storage, and therefore TCES-based technology can be used for both long-term (weeks to months, even years) and short-term (hours to days) applications, as well as for both heating and cooling applications.

[0008] The core of TCES-based TES technology is thermochemical material (TCM), which has a high energy density, allowing a relatively large amount of energy to be stored in a relatively small mass / volume of material.

[0009] There are many TCMs, and salt hydrates are a class of materials with many potential applications, particularly for cryogenic and intermediate temperature ranges. However, salt hydrates in their pure form generally face two technical challenges:

[0010] a) They have low thermal conductivity, resulting in heat transfer limitations in thermochemical processes.

[0011] b) Almost all of these salts become structurally unstable after just a few thermal cycles due to one or more of deliquescence, disintegration, densification, agglomeration, and pore / channel blockage, resulting in mass transfer limited thermochemical processes.

[0012] Both challenges limit the kinetics of the thermochemical process; the second challenge leads to poor cyclability and degradation of system performance over time. Both challenges also make TCES-based TES less controllable than other schemes.

[0013] For example, CaCl 2 6H 2 O and LiCl·H 2 O is susceptible to deliquesce. These TCMs are only able to maintain their form in very low relative humidity environments, which limits their available applications.

[0014] MgCl 2 6H 2 O has a high theoretical energy density (about 3GJ / m 3 ) and good reaction kinetics, however, structural instability often occurs after several hydration and dehydration cycles, leading to a decrease in energy density and system blockage. In addition, it has been reported that harmful gas HCl is formed when heated above 130 °C.

[0015] MgSO 4 7H 2 O (epsom salt) due to its high theoretical energy density (about 2.8GJ / m 3 However, despite extensive efforts, little progress has been made in achieving high energy density.

[0016] The above issues also affect other categories of TCMs. One of the main common challenges hindering the commercialization of TCES technology is the material stability (especially after thermal cycling) and the kinetic controllability of the charging and releasing processes.

[0017] To overcome these challenges, efforts have been made to investigate the use of structural / host materials to house TCMs. Such materials containing hydrate salts may be referred to as composite TCMs.

[0018] The use of porous matrices as support materials for TCMs has been reported, which provide water vapor transport channels, where the host matrix acts as a semipermeable container that retains the salt and allows water vapor to pass through mechanisms such as diffusion due to concentration gradients and migration due to temperature gradients. This enhances the dehydration / hydration kinetics and conversion rates, and provides better stability and recyclability, resulting in improved performance of salt hydrates.

[0019] In recent years, the use of clay, zeolite, MgO-modified zeolite, silica gel, activated carbon, vermiculite, porous glass and attapulgite has been reported, and salts have been inserted into these host materials using an impregnation method. However, the disclosed matrix materials have a rigid structure, which limits the mechanical stability of the material during thermal cycling due to the expansion / contraction of the salt hydrate particles during hydration / dehydration. In addition, the amount of salt impregnated into the structure is usually limited, thus providing a low energy density. In addition, the cyclability of this type of composite material is poor, usually less than 10 cycles.

[0020] Many, if not all, reported methods for preparing composite TCMs are based on impregnation, where a porous scaffold is immersed in a saturated saline solution that penetrates the pore structure of the scaffold and the impregnated matrix is ​​subsequently dried in an oven set at a certain temperature. However, impregnation is energy intensive and the composites produced have poor mechanical strength and typically have low TCM content, resulting in low energy density and poor recyclability. In addition, impregnation can take a lot of time due to limitations in the pore structure of the scaffold and the surface area to volume ratio.

[0021] An alternative approach uses polymer macroporous foams as the porous matrix for the salt, with reported salt additions as high as about 70%. In this approach, the TCM material is mixed with a polymer precursor and a foaming polymer (e.g., silicone foam) formed by the addition of a catalyst. Although the foam structure is elastic and thus may be able to withstand the expansion / contraction forces during cyclic conditions, the volumetric energy density of the prepared composites is relatively low, ranging from 0.26 GJ / m at 50 wt% TCM to 0.10 GJ / m at 1.5 wt%. 3 0.48 GJ / m at 70 wt% TCM 3 (Piperopoulos E et al., Appl Sci, 2020, 10). In addition, the preparation process is chemical in nature and requires catalysts, which is disadvantageous and generally expensive.

[0022] It would be advantageous to provide a TCM having a high energy density (eg, volumetric energy density and / or gravimetric energy density) and exhibiting sufficient mechanical stability to withstand multiple operating cycles.

[0023] It is therefore an object of the present invention to provide thermochemical materials that exhibit one or more of improved material stability (especially after multiple operating cycles), high energy density, and controllability of charging and discharging kinetics.

[0024] It would also be beneficial to provide a TCM that has low production costs, low energy consumption during production, can use abundant materials, and / or has improved performance compared to other TCMs due to one or both of favorable heat and mass transfer rates and reaction kinetics.

[0025] Thus, according to a first aspect of the present invention there is provided a thermochemical material comprising a mixture of particles of a hydrated or hydratable inorganic salt and an inorganic host material.

[0026] The inorganic host material can be porous, and advantageously, the porous host material serves as a support material for providing intra-particle and inter-particle channels for water vapor transmission. In this way, the porous host material can improve the performance of hydration or hydratable inorganic salts by providing other transmission channels for the mass transfer of reactants, increasing the surface area of ​​heat transfer and reaction, and allowing the volume change of salt and thus allowing cyclability to improve. Additionally or alternatively, the porous inorganic host material can be sufficiently porous to accommodate at least a portion of hydration or hydratable inorganic salts in its pores, so that the material can have a high energy storage density.

[0027] The thermochemical material may be in pellet form, tablet form, granulate form, or extruded form.

[0028] The hydrated or hydratable inorganic salt may be a hygroscopic salt such as CaCl 2 MgCl 2 MgSO 4 , SrBr 2 For example, the hydrated or hydratable inorganic salt may be selected from MgSO 4 7H 2 O.K 2 CO 3 ·H 2 O, CaSO 4 ·2H 2 O or SrBr 2 6H 2 O or a mixture thereof.

[0029] Additionally or alternatively, the hydrated or hydratable inorganic salt may be selected from aluminum sulfate (e.g., Al 2 (SO 4 ) 3 6H 2 O), copper sulfate (e.g., CuSO 4 ·5H 2O), lithium sulfate (e.g., Li 2 SO 4 ·H 2 O), calcium hydroxide (Ca(OH) 2 )、Magnesium hydroxide (Mg(OH) 2 ·H 2 O), iron oxides (e.g., Fe(OH)), sodium sulfide (e.g., Na 2 S.5H 2 O) and mixtures of one or more thereof, with or without one or more of the above-mentioned hygroscopic salts.

[0030] Advantageously, the inorganic host material not only provides a structure to contain the hydrated or hydratable inorganic salt, prevent its leakage and improve mechanical strength and thermal cyclability, but also improves the dehydration and rehydration kinetics and thus improves the overall material properties compared to pure salt hydrates.

[0031] The volume energy density of hydrated or hydratable inorganic salts can be higher than 0.6 GJ / m 3 , 0.7GJ / m 3 , 0.8GJ / m 3 , 0.9GJ / m 3 , 1.0GJ / m 3 , 1.1GJ / m 3 , 1.2GJ / m 3 , 1.3GJ / m 3 , 1.4GJ / m 3 , 1.5GJ / m 3 , 1.6GJ / m 3 , 1.7GJ / m 3 , 1.8GJ / m 3 , 1.9GJ / m 3 , 2.0GJ / m 3 , 2.1GJ / m 3 , 2.2GJ / m 3 , 2.3GJ / m 3 , 2.4GJ / m 3 , 2.5GJ / m 3 , 2.6GJ / m 3 , 2.7GJ / m 3 , 2.8GJ / m 3 , 2.9GJ / m 3 、3.0GJ / m 3 、3.1GJ / m 3 or 3.2GJ / m 3 The volume energy density of hydrated or hydratable inorganic salts can be 0.9 GJ / m 3 Up to 3.2GJ / m3 , preferably above 1.0 GJ / m 3 , 1.1GJ / m 3 , 1.2GJ / m 3 , 1.3GJ / m 3 , 1.4GJ / m 3 , 1.5GJ / m 3 , 1.6GJ / m 3 , 1.7GJ / m 3 , 1.8GJ / m 3 , 1.9GJ / m 3 , 2.0GJ / m 3 , 2.1GJ / m 3 , 2.2GJ / m 3 Up to 3.2GJ / m 3 within the range.

[0032] The hydrated or hydratable inorganic salt may be selected based on one or more of theoretical energy density, temperature of hydration and dehydration, chemical stability, corrosivity and / or toxicity, end-use requirements, abundance, and cost.

[0033] Hydration or hydratable inorganic salt can be a particle, such as a particle in nanoparticle, submicron and micron range.Preferably, the inorganic host material is porous, and hydration or hydratable inorganic salt, such as at least some of hydration or hydratable inorganic salt particles are provided in the hole of the inorganic host material, and some of the salt particles in the gap between the inorganic host materials.Therefore, the salt particles can be located in the particle of the host material and / or between the particles.In embodiments, the inorganic host material can form the agglomerate of primary particles, and hydration or hydratable salt material can be located in the hole or the void space of the agglomerate.

[0034] The hydrated or hydratable inorganic salt may be present in a mass percentage of greater than 10 wt %, for example greater than 15 wt %, 20 wt %, 25 wt %, 30 wt %, 35 wt %, 40 wt %, 45 wt %, 50 wt %, 55 wt %, 60 wt %, 65 wt %, 70 wt %, 75 wt %, 80 wt % of the composite thermochemical material. For example, the hydrated or hydratable inorganic salt can be present in a mass percentage of 10% to 60% by weight of the thermochemical material, such as from 10%, 15%, 20%, 25%, 30%, 35%, 50%, 45%, 50%, 55% or 60% by weight of salt hydrate, such as any of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% to any of 80%, 75%, 70%, 60%, 55%, 50%, 45%, 40%, 35%, 30%, 25%, 20%, 15% by weight.

[0035] The inorganic host material may be selected from, for example, vermiculite, zeolite, MgO, diatomaceous earth, clay, silica gel, porous glass, attapulgite, graphite, activated carbon and / or combinations thereof. Advantageously, the inorganic host material is cheap and has or can be manufactured to have an excellent pore structure.

[0036] Thermochemical materials can include less than 90% by weight, such as less than 85%, 80%, 75%, 70%, 65%, 60%, 55%, 50%, 45%, 40%, 35%, 30%, 25%, 20% by weight of inorganic host materials. The inorganic host material can be present in a range of 20% to 90% by weight, such as 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, or 90% by weight.

[0037] Preferably, the inorganic host material is present as a minority (weight %) component of the thermochemical material. Preferably, the hydrated or hydratable salt is present as a majority (weight %) component of the thermochemical material.

[0038] The particle size of the particles of the inorganic host material can be in the range of 0.01 mm to 10 mm, for example 0.02 mm, 0.03 mm, 0.4 mm or 0.05 mm to 10.0 mm, 9.0 mm, 8.0 mm, 7.0 mm, 6.0 mm, 5.0 mm, 4.0 mm, 3.0 mm, 2.0 mm, 1.0 mm. The particle size of the particles of the inorganic host material can be in the range of 0.08 mm to 1 mm.

[0039] The thermochemical material may also contain a binder. Advantageously, the addition of a binder may help to form a shape-stable form. In addition, the addition of a binder may enhance the mechanical strength of the thermochemical material during the charge / discharge cycle.

[0040] The binder can be a high temperature / hygroscopic polymer binder. The binder can be selected from one or more of polyvinyl pyrrolidone (polyvidone PVP), starch, alginate, casein, cellulose binders such as hydroxypropyl methylcellulose (HPMC), polyvinyl acetate (PVA), polyacrylic acid, etc. The binder can preferably be a water-soluble hygroscopic polymer.

[0041] If the binder is hygroscopic, it can help the thermochemical material to attract and hold / store more water molecules (for facilitating the thermochemical process), thus providing a water buffering and balancing function during the thermochemical reaction / adsorption process.

[0042] Advantageously, the addition of binders has been shown to enhance TCM performance while having little impact on the thermophysical properties of the thermochemical material.

[0043] The percentage of binding agent can be up to 5 weight % of thermochemical material, for example, in the range of 0.25 weight % to 5 weight %, for example, 0.5 weight % to 3 weight %. For example, the mass percentage of binding agent can be 0.25 weight %, 0.5 weight %, 0.75 weight %, 1.0 weight %, 1.25 weight %, 1.5 weight %, 1.75 weight %, 2 weight %, 2.25 weight %, 2.5 weight %, 2.75 weight %, 3 weight %, 3.25 weight %, 3.5 weight %, 3.75 weight %, 4 weight %, 4.25 weight %, 4.5 weight %, 4.75 weight % or 5 weight %. In an embodiment, binding agent can exist as a solution. When using a binding agent solution, the weight percentage of the above-mentioned binding agent relates to the binding agent itself, rather than the binding agent solution.

[0044] A hydrated or hydratable salt may have a stoichiometry of multiple water molecules to hydrate the salt molecule. The dehydration reaction of a hydrated or hydratable salt may be carried out in a stepwise manner.

[0045] The formulation may also contain a flow aid to enhance mixing of the salt and host material particles and reduce caking / agglomeration. The flow aid may be a fumed silica, for example selected from Fumed silica (available from Lawrence Industries Ltd of Tamworth, UK), and Precipitated silica (available from Evonik Industries AG, Essen, Germany). The weight percentage of flow aids may be 0.01% to 5.0%.

[0046] The operating temperature of the thermochemical material, e.g., the reaction temperature, may be from 20° C. to 500° C. In one embodiment, the operating temperature may be at or below 200° C., 175° C., or 150° C., such as at or below 145° C., 140° C., 145° C., 130° C., 135° C., 120° C., 125° C., or 120° C. For example, the operating / reaction temperature may be 150° C., 149° C., 148° C., 147° C., 146° C., 145° C., 143° C., 142° C., 141° C., 140° C., 139° C., 138° C., 137° C., 136° C., 135° C., 134° C., 133° C., 132° C., 131° C., 130° C., 129° C., 128° C., 127° C., 126° C., 125° C., 124° C., 123° C., 122° C., 121° C., 120° C., 119° C., 118° C., 117° C., 116° C. or 115° C. This is advantageous because 150° C. is known to be a temperature achievable by solar collectors and is also within the temperature range of industrial waste heat.

[0047] The volume energy density of thermochemical materials based on reaction enthalpy can be 80 MJ / m 3 Up to 2000MJ / m 3 , for example 90MJ / m 3 Up to 800MJ / m 3 , or 100MJ / m 3 Up to 2000MJ / m 3 , for example 103MJ / m 3 Up to 2000MJ / m 3 The heat of reaction can increase as the pore size of the inorganic host material decreases.

[0048] The mass energy density of the thermochemical material may be in the range of 400 J / g to 1500 J / g, eg, 600 J / g to 1400 J / g, 600 J / g to 1000 J / g, 650 J / g to 900 J / g, or 658 J / g to 758 J / g.

[0049] Advantageously, the methods of the present invention can enable thermochemical materials to reach > about 1000 kJ / g (> about 1 GJ / m 3 or 280KWh / m 3 )’s energy density.

[0050] Advantageously, the thermochemical material is non-toxic.

[0051] Thermochemical materials can be used to store industrial waste heat and / or renewable heat from solar and / or wind energy for building applications such as space heating, cooling, hot water supply, hot air supply and / or steam supply.

[0052] Thermochemical materials could be used in next-generation air conditioning systems, partially replacing refrigerant-based vapor compression technology.

[0053] Therefore, a second aspect of the present invention provides a method for producing a thermochemical material, the method comprising:

[0054] a) mixing, preferably dry mixing, a salt hydrate and an inorganic host material; and

[0055] b) Shaping / compacting the dry powder mixture into a shape-stable body. The composite TCM body may be in the form of pellets, granules or extrudates.

[0056] Another aspect of the present invention provides a method for forming a composite thermochemical material, the method comprising providing an inorganic host material and providing a hydrated or hydratable inorganic salt, mixing the inorganic host material and the hydrated or hydratable inorganic salt under low relative humidity conditions to form a mixture, allowing or causing at least a portion of the hydrated or hydratable inorganic salt to enter the pores of the inorganic host material, and forming the mixture into a shaped body.

[0057] Advantageously, dry mixing (i.e., under relatively low humidity conditions) overcomes the problems associated with wet processes, such as corrosion, waste streams, and high energy consumption due to drying. In this specification, relatively low humidity conditions mean ambient conditions or conditions below which a hydrated or hydratable inorganic salt would deliquesce.

[0058] Advantageously, the method does not require a washing stage, ie, the entire material does not need to be washed after mixing. Instead, the salt hydrate is compacted with the inorganic host material into a TCM composite formulation.

[0059] Step (a) may comprise adding a salt hydrate at a ratio of 10 wt % to 80 wt %, such as 10 wt %, 15 wt %, 20 wt %, 25 wt %, 30 wt %, 35 wt %, 50 wt %, 45 wt %, 50 wt %, 55 wt %, 60 wt %, 65 wt %, 70 wt %, 75 wt % or 80 wt % of the salt hydrate. The salt hydrate may be a hygroscopic salt in a dehydrated form, such as CaCl2 MgCl 2 MgSO 4 , SrBr 2 The salt hydrate may be MgSO in its hydrated form 4 7H 2 O. KCO 3 1.5H 2 O, CaSO 4 ·2H 2 O or SrBr 2 ·H 2 O.

[0060] Step (a) may include adding an inorganic host material in the range of 20 wt % to 90 wt %, for example 20 wt %, 25 wt %, 30 wt %, 35 wt %, 40 wt %, 45 wt %, 50 wt %, 55 wt %, 60 wt %, 65 wt %, 70 wt %, 75 wt %, 80 wt %, 85 wt % or 90 wt % of the host material. The host material may be porous on a single particle scale, such as vermiculite, zeolite and diatomaceous earth; non-porous on a particle scale, such as some MgO and graphite; and / or combinations thereof. The inorganic host material is in powder form, wherein the pores of the porous host material consist of both inter-particle pores (between particles) and intra-particle pores (inside a single particle), while the pores of the non-porous host material only contain inter-particle pores. The median pore size / pore diameter of the porous host material may be in the range of 7 nm to 500 μm.

[0061] The method may include pre-grinding the inorganic host material before step (a), for example using a pulverizer, a pin mill and / or a ball mill. Pre-grinding the inorganic host material may obtain an optimal size of the porous host material in the range of 0.01 mm to 1.5 mm, for example 0.02 mm, 0.05 mm, 0.09 mm, 0.12 mm, 0.25 mm, 0.5 mm, 0.75 mm, 1.00 mm, 1.5 mm, or a mixture of different sizes.

[0062] For low moisture sensitive formulations and non-moisture sensitive formulations, the method may include grinding the mixture from step (a) into small particles, such as microparticles, for example in the range of 7 nm to 500 μm. In this way, the salt particles can be reduced to a small particle size (e.g., 5 nm to 500 μm) to fit into the inter-particle pores and intra-particle pores of the porous host material.

[0063] The method may include diffusing the salt hydrate into the structure of the host material, for example under deliquescent conditions.

[0064] Step (b) can be carried out by two main processes: batch process and continuous process.

[0065] Batch processes can use compacting devices such as tablet presses, granulators, hydraulic presses or briquette presses. A small amount of water can be added to help shape stability and lubrication. The percentage of water added is in the range of 0% to 8% by mass, for example 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 4%, 5%, 7%, 8%.

[0066] Continuous processes use an extrusion device, such as a single screw extruder or a twin screw extruder.

[0067] Step (b) may include heating to a temperature below 150°C, e.g., below 145°C, 140°C, 135°C, 130°C, 125°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, 90°C, 85°C or 80°C to dry the composite TCM body.

[0068] The method may further include adding a binder, such as a high temperature / hygroscopic polymer binder. The binder may be polyvinyl pyrrolidone (PVP), a water-soluble hygroscopic polymer with good bonding properties. The addition of the binder may include (i) dissolving the binder in water, such as a 1 wt % to 15 wt % solution, and (ii) adding a small amount of the binder solution to the mixture in step (a), such as 0.1 wt % to 5 wt % relative to the TCM composite material.

[0069] The method may further comprise adding a flow aid to the mixture in step (a). The flow aid may be selected from Fumed silica and Precipitated silica. The percentage of flow aid may be from 0.01% to 5.0%.

[0070] The batch process using a tabletting device in step (b) can include using a compression loading speed of 30 mm / min to 5 mm / min, such as 20 mm / min to 10 mm / min, such as 30 mm / min, 25 mm / min, 20 mm / min, 15 mm / min, 10 mm / min or 5 mm / min. Compression of the mixture can include using a stress holding time of 0.5 to 5 minutes, such as 1 to 3 minutes, such as 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5 minutes. Compression of the mixture may include employing a pressure of 1 MPa to 100 MPa, for example 1 MPa, 5 MPa, 10 MPa, 15 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 65 MPa, 70 MPa, 75 MPa, 80 MPa, 85 MPa, 90 MPa or 100 MPa.

[0071] By using slow loading rates and long stress / pressure hold times during compression, the structural stabilization of the composite TCM body can be improved.

[0072] The method may further comprise granulating the mixture of the host material and the salt hydrate before or during step (b). The granulate produced in step (b) may be used as one of the TCM body forms.

[0073] Advantageously, the methods of the present invention can enable thermochemical materials to reach > about 1000 kJ / g (> about 1 GJ / m 3 or 280KWh / m 3 )’s energy density.

[0074] Advantageously, the manufacturing method of the present invention enables customization of the shape and / or size of thermochemical material modules having strong mechanical strength and good stability; and is easily scaled up.

[0075] Advantageously, the methods of the present invention form bodies of thermochemical materials having substantially increased mechanical strength, reduced volume changes, reduced agglomeration and leakage, improved hydration / dehydration kinetics, and greatly improved thermal stability and cyclability compared to the prior art.

[0076] Within the scope of the present application, it is expressly intended that the various aspects, embodiments, examples and alternatives set forth in the preceding paragraphs, in the claims and / or in the following description and drawings, in particular their individual features, may be adopted independently or in any combination. That is, all embodiments and / or the features of any embodiment may be combined in any manner and / or combination unless such features are incompatible. For the avoidance of doubt, the terms "may", "and / or", "such as", "for example" and any similar terms as used herein should be interpreted as non-restrictive, and therefore no features described in this manner need be presented. In fact, any combination of optional features is expressly contemplated without departing from the scope of the present invention, whether or not these are explicitly claimed for protection. The applicant reserves the right to change any initially filed claims or to submit any new claims accordingly, including the right to amend any initially filed claims to be subordinate to any other claims and / or to merge any features of any other claims, although protection was not initially claimed in this manner.

[0077] The present invention will now be described by way of example only and with reference to the accompanying drawings, in which:

[0078] Figure 1 A schematic diagram showing the working principle of thermochemical energy storage using a composite thermochemical material module;

[0079] Figure 2 Composite MgSO using batch compaction process 4 7H 2 Schematic diagram of the O-body manufacturing method;

[0080] Figure 3 To show the MgSO 4 7H 2 Figure 2 shows the X-ray diffraction (XRD) curve of O dehydration;

[0081] Figure 4 To show the MgSO 4 7H 2 A graph of the differential scanning calorimetry (DSC) curve of O dehydration;

[0082] Figures 5A to 5C MgSO 4 7H 2 Simultaneous Thermal Analysis (STA) and DSC measurement results of O dehydration;

[0083] Figure 6 To show that MgSO 4 7H 2 Diagram of the desorption process of O followed by the adsorption process;

[0084] Figure 7 To show the effect of temperature on MgSO 4 7H 2 O Diagram of the effects of dehydration and hydration;

[0085] Figure 8 To show that MgSO 4 7H 2 O Plot of dehydration / hydration behavior;

[0086] Fig. 9 To show the MgSO 4 7H 2 O graph of dehydration curve;

[0087] Fig.10 A to 10D show the MgSO after different thermal cycles 4 7H 2 Scanning electron microscopy (SEM) images of the shape and morphology of the salt crystals of O;

[0088] Fig.11 To show different MgSO 4 7H 2 Plot of DSC heat flow data during dehydration of O composites;

[0089] Fig.12 To show the effect of particle size of the host material on MgSO 4 7H 2 O Plot of the effect of heat flow measured during dehydration of the composite material;

[0090] Fig.13 To show the measured MgSO in pellet and powder form under dehydration 4 7H 2 Plot of DSC heat flow of O / vermiculite composites;

[0091] Fig.14 To show that MgSO 4 7H 2 Figure 2. Dynamic Vapor Sorption (DVS) measurement results of desorption (dehydration) and adsorption (hydration) processes of O / MgO composites.

[0092] Fig.15 To show that MgSO 4 7H 2 Figure 2. (DVS) measurement results of the desorption (dehydration) and adsorption (hydration) processes of O / vermiculite composites within one cycle.

[0093] Fig.16 To show the effect of vermiculite particle size on MgSO4 7H 2 Plot of the effect of hydration and dehydration of O / vermiculite composites over two cycles;

[0094] Fig.17 To show 60 wt% MgSO 4 7H 2 Plots of heat flow (DSC measurement) and mass change (TG measurement) during dehydration and hydration of O / MgO composites over 35 cycles;

[0095] Fig.18 MgSO 4 7H 2 Plots of heat flow (DSC measurement) and mass change (TG measurement) during dehydration and hydration of O / vermiculite composites over 35 cycles;

[0096] Fig.19 To show 60 wt% MgSO 4 7H 2 Figure 2 DSC curves of O / 0.5 mm vermiculite composite after different cycles;

[0097] Fig. 20 A and 20B are MgSO 4 7H 2 Images of O composites before and after STA cycles;

[0098] Fig.21 A to 21E are MgSO 4 7H 2 SEM images of O / MgO composites before and after thermal cycling in STA.

[0099] Fig. 22 A to 22D are MgSO 4 7H 2 SEM images of O / vermiculite composites before and after thermal cycling in STA;

[0100] Fig.23 A to 23D are 60 wt% MgSO 4 7H 2 Images of O / 0.5 mm vermiculite composite pellets after different cycles in the humidity chamber;

[0101] Fig.24 A to 24C are 60 wt% MgSO prepared with different compression pressures. 4 7H 2 X-ray tomography (XRT) images of O / vermiculite composite pellets after 10 cycles in a humidity chamber;

[0102] Fig.2560 wt% MgSO 4 7H 2 O / Images of vermiculite pellets after different cycles in the humidity chamber;

[0103] Fig.26 A and 26B are 60 wt% MgSO 4 7H 2 O / XRT images of vermiculite pellets after 16 cycles in the humidity chamber;

[0104] Fig. 27 60 wt% MgSO 4 7H 2 O / Graph of XRD curves of vermiculite pellets after different cycles in a humidity chamber;

[0105] Fig.28 60 wt% MgSO 4 7H 2 O / Graph of DSC heat flow measurement data of vermiculite pellets after different cycles in a humidity chamber;

[0106] Fig.29 60 wt% MgSO with 0.5 to 3 wt% PVP 4 7H 2 Images of the O / vermiculite composite after different cycles in the humidity chamber showing a 2% optimum; and

[0107] Fig.30 MgSO with 2 wt% PVP binder 4 7H 2 Plot of the dehydration / hydration and cycling behavior of O / vermiculite composites.

[0108] Schematic representation of the working principle of salt hydrate composites during dehydration (desorption) and hydration (adsorption) processes. Figure 1 exist Figure 1 The porous matrix (e.g., vermiculite, zeolite, MgO, etc.) holds a hygroscopic salt (e.g., CaCl 2 MgCl 2 MgSO 4 , SrBr 2 etc.) to provide an enlarged surface and sites for dehydration / hydration reactions, limit the effects of salt deliquescence, provide pathways for mass transfer, and enhance mechanical properties and heat transfer.

[0109] Heat is stored in the desorption (dehydration) process by destroying the binding force between the adsorbent (salt hydrate) and the adsorbate (water). In this process, the salt hydrate is converted into partially dehydrated salt or anhydrous salt, and the water is condensed (recovering condensation heat). Salt and water can be stored separately at ambient temperature with almost no energy loss. The matrix is ​​used to hold the adsorbent, prevent leakage, enhance heat and mass transfer, and enhance reaction kinetics and mechanical properties. When the charged composite material is exposed to humid air, heat is released on demand through the adsorption (hydration) process, causing an exothermic reaction. Repeat the above dehydration and hydration process to store and release heat in a cyclic manner. By utilizing this principle, renewable energy (such as solar energy, wind energy and biomass energy), industrial waste heat and non-peak electricity can be converted and stored when supply exceeds demand, so as to be used when demand exceeds supply, such as meeting winter peak heating demand and summer peak cooling demand. Since there is almost zero loss during storage, the storage process can be long-term (months and years), which can also meet short-term (hours) and medium-term (days and weeks) needs.

[0110] In the following, MgSO 4 7H 2 O as an exemplary salt and MgO and vermiculite as exemplary host materials to illustrate the experimental procedures and characterization methods:

[0111] experiment

[0112] 1.Raw materials

[0113] Reagent grade powders of magnesium sulfate heptahydrate (VWR, CAS 10034-99-8, 99.5% purity) with a particle size in the range of 0.2 mm to 0.5 mm, magnesium oxide (Merck, CAS 1309-48-4, ≥ 99% purity) with a particle size in the range of 5 μm to 10 μm, and vermiculite (Merck, CAS 1318-00-9) with a particle size in the range of 2 mm to 10 mm were used. The coarse vermiculite material was crushed before the experiment to obtain particles with different sizes in the range of 0.08 mm to 1 mm.

[0114] 2. Composite TCM Formation and Fabrication

[0115] Reference Figure 2 , showing the process of formulating and manufacturing composite materials using a batch compaction process Figure 2 The steps are as follows:

[0116] a) using a pulverizer or alternative grinder 21 to pulverize an inorganic host material 20 such as vermiculite into a fine powder 22 of various particle sizes (typically 80 μm to 1 mm) (step 2A);

[0117] b) by adding MgSO4 7H 2 O 23 (e.g., at a mass percentage of 10 wt% to 80 wt%), and by dry-mixing the two materials 22, 23 using a mixer, a predetermined amount (e.g., 5 g to 10 g) of thermochemical material 24 is prepared (step 2B). On a laboratory scale, this can be achieved using a mortar. The mixing or grinding action breaks the thermochemical material into smaller particles, at least some of which will enter the pores in the powder of the host material;

[0118] c) shaping the mixture 24 under laboratory conditions using a press 25 at various pressures (e.g. 20 MPa) to form composite TCM modules or pellets 26, e.g. 13 mm diameter disc-shaped modules (step 2C); and

[0119] d) Store the composite TCM module / pellet 26 in a sealed container such as glass.

[0120] 3. Material Characterization

[0121] X-ray diffraction (XRD)

[0122] XRD measurements were performed to determine the MgSO 4 .7H 2 Crystallinity and phase changes during the O dehydration process. XRD patterns were collected by a Bruker D8Advance with an in-situ high temperature stage using 40 kV, 40 mA and a Cu Kα1+Kα2 radiation source. Scans were recorded at a scan speed of 0.2 sec / step using a step size of 0.02° in the 2θ range of 10° to 40°. The sample was slowly heated from 25°C to 300°C at a heating rate of 1°C / min to avoid the measurement peak from shifting to higher temperatures, and then rapidly cooled from 300°C to 25°C at a cooling rate of 12°C / min. Diffraction patterns were recorded every 10°C in heating mode. The experimental raw patterns were analyzed using Bruker EVA evaluation software with the JCPDS-ICDD PDF 2016 database.

[0123] Scanning electron microscopy (SEM)

[0124] SEM measurements were performed to determine the MgSO 4 Morphological changes and modifications of hydrates after cyclic dehydration and hydration. The morphology of the samples was obtained by using a Hitch TM3030 benchtop SEM at 15 kV.

[0125] X-ray Tomography Micro-CT (XRT)

[0126] XRT measurements with a Bruker Skyscan 2211 with a CMOS flat panel detector to investigate MgSO4 The internal structure of the composite material after dehydration and hydration cycles. XRT scanning was performed using 180 kVp accelerating voltage, 120 μA current and Cu filter at an exposure time of 250 milliseconds. Images were recorded using a rotation step of 0.2 ° / second. Images acquired from different angles allowed the reconstruction of the 2D and 3D structures of the composite material using Bruker XRT reconstruction processing software.

[0127] Mercury porosimetry

[0128] The porosity of porous vermiculite, MgO and salt composites was characterized using mercury intrusion porosimetry. Data was collected using an Autopore IV 9500 porosimeter (Micrometrics GmbH, Germany), which allows the measurement of pore sizes in the range of 0.003 μm to 360 μm. Both low-pressure and high-pressure tanks were usually analyzed using 50 μm Hg vacuum pressure, 5 minutes vacuum time, 0.49 psia mercury filling pressure and 5 seconds equilibrium time. After vacuum pretreatment for 2 hours at a temperature of 150 ° C, additional physical adsorption measurements were performed on Micromeritics TriStar II Plus by nitrogen adsorption at 196 ° C to determine the surface area and volume of the pores with diameter <13 nm (the lower limit of Hg porosimeter measurement). The BET method was used based on 0.02 p / p 0 To 0.20p / p 0 Surface area was calculated from adsorption data over a range of partial pressures. Pore size analysis was performed using the Barrett-Joyner-Halenda method.

[0129] 4. Analysis of Dehydration / Hydration Kinetics and Recyclability

[0130] Thermal analysis was performed to understand the dehydration and hydration kinetics and cyclability of TCM. Three thermal analysis techniques were used: DSC, STA, STA with pressure and humidity control unit, and DVS adsorption analysis:

[0131] Differential Scanning Calorimetry (DSC)

[0132] DSC measures the heat flow change (absorption or release) as a function of temperature and time. MettlerToledo DSC3+ is used in this work, which operates at a temperature range of -70°C to 700°C. In a typical experiment, the sample is dehydrated by heating from 25°C to 150°C at a heating rate of 10°C / minute. It is followed by a holding period of 45 minutes at 150°C to ensure that each part of the sample is dehydrated to the same extent. All measurements are carried out under a flowing nitrogen atmosphere with a flow rate of 50ml / minute by using a sample of about 5mg. The sample pan used in these experiments is a 40μl standard aluminum crucible with a lid. The heat flow measured during dehydration is used to quantify the thermal storage capacity of the material. Additional experiments are carried out at heating rates of 1°C / minute, 2°C / minute, 5°C / minute and 10°C / minute to study the effect of heating rate on the dehydration behavior of salt hydrate materials.

[0133] Simultaneous Thermal Analysis (STA)

[0134] STA is a system combined with DSC and thermogravimetric analysis (TGA) for measuring heat flow and mass change as a function of temperature or time. Dehydration measurements are performed using a Netzsch STA409 with a standard silicon carbide (SiC) furnace. Measurements are performed under atmospheric pressure (1atm) with about 10mg sample at a flow rate of 50ml / min of flowing nitrogen. Typical measurements include raising the temperature of the sample from 25°C to 320°C, followed by cooling the sample to 25°C, wherein the rate of both heating and cooling is 5°C / min. The sample pan is a 40μl standard aluminum crucible with a lid. Use the heat flow and mass change measured during dehydration to understand the thermochemical process and quantify the thermal storage capacity of the material.

[0135] Simultaneous Thermal Analysis (STA) with Humidity Control

[0136] The dehydration, hydration and cyclability of thermochemical energy storage materials and their composite materials were studied using STA equipped with a humidity control unit. Low-pressure LINSEIE STA equipment was used in this work. Both dehydration and hydration measurements were performed at atmospheric pressure by exposing about 20 mg of sample to an air atmosphere with a flow rate of 100 ml / min. Air was used here to ensure that the cycle test was carried out under conditions similar to actual applications. During the hydration experiment, a 70 μl platinum crucible without a lid was used. To this end, the sample was first dehydrated by heating from 25 ° C to 150 ° C at a heating rate of 1 ° C / min. The sample was then kept at 150 ° C for 60 minutes to ensure that every part of the sample was dehydrated. Finally, the sample was cooled from 150 ° C to 35 ° C at a cooling rate of 2 ° C / min. The dehydrated sample was then kept for 30 minutes and then rehydrated for 3 to 6 hours at a constant temperature of 35 ° C and a relative humidity (RH) of 85%. The heat flow and mass change measured during the dehydration and hydration process were used to quantify the thermal storage capacity of the material during the adsorption cycle. Different rehydration temperatures of 25°C, 35°C, 45°C and 55°C were used to understand the effect of temperature on the rehydration kinetics, with the ultimate goal of finding the most suitable conditions for the application.

[0137] Dynamic Vapor Sorption (DVS)

[0138] Use DVS Advance from Surface Measurement Systems Ltd to study dynamic vapor / water desorption (dehydration) and adsorption (hydration) processes. The sample pan used is 200 μl stainless steel, which can accommodate samples of 30 mg to 50 mg scale. In a typical dehydration process, the sample is heated from 25 ° C to 135 ° C at a heating rate of 1 ° C / minute, and then the sample is kept at 135 ° C for 60 minutes for complete dehydration. Then the sample is cooled from 135 ° C to 35 ° C at a cooling rate of 2 ° C / minute, and then the sample is kept at 35 ° C for 30 minutes. Sample hydration is carried out at 35 ° C and 85% RH for 12 hours to 16 hours until equilibrium is reached. These measurements are carried out at atmospheric pressure by exposing the sample to a nitrogen gas flow of 200 ml / minute. The mass change as a function of time is collected during the desorption (dehydration) and adsorption (hydration) processes.

[0139] The invention will be further illustrated by reference to the following non-limiting examples.

[0140] Example 1 -Pure MgSO 4 7H 2 Dehydration of O

[0141] Kinetics of dehydration and hydration reactions for MgSO 4 7H 2The application of O as a TCM storage material is important. The kinetic parameters of these reactions can be used to help understand the reaction mechanism and obtain the optimal formulation of TCM composites.

[0142] Typically, the dehydration reaction proceeds stepwise through a series of intermediate reactions including the decomposition of one phase and the formation of a new phase. Prior art studies have reported that the main dehydration step is completed at about 150 °C to produce MgSO 4 ·H 2 O. However, many different intermediate phases have also been reported, such as MgSO 4 ·5H 2 O、MgSO 4 ·3H 2 O and MgSO 4 ·2H 2 O, and each mol of MgSO 4 1.25 mol to 1.5 mol H 2 A less clear intermediate of O. The dehydration was also found to vary strongly depending on the experimental conditions.

[0143] Now refer to Figure 3 , showing the original MgSO 4 7H 2 XRD diffraction patterns of O at different temperature points from 25°C to 300°C during heating and then cooling to 25°C.

[0144] XRD data showed that MgSO 4 7H 2 The dehydration of O occurs in three different stages divided by the temperatures of 44°C, 80°C and 276°C:

[0145] Stage 1 - MgSO 4 7H 2 The initial crystalline phase of O (at 25 °C) dehydrates upon heating to form MgSO at 28 °C. 4 7H 2 O and MgSO 4 6H 2 O crystalline phases, further heating resulted in only MgSO 4 6H 2 O crystalline phase.

[0146] Stage 2 - Further heating leads to MgSO 4 6H 2 O gradually dehydrates to form MgSO at 80 °C 4 ·nH 2 O. No peaks were observed in the XRD pattern between 80 °C and 276 °C, indicating that MgSO 4 ·nH2 O is an amorphous phase.

[0147] Stage 3 - Further heating to 300°C to obtain anhydrous MgSO 4 Crystalline phase.

[0148] For the intermediate hydrated phase MgSO 4 ·nH 2 O, n can be from 5 to 0, such as 5, 4, 2.5, 2, 1 or 0.5. Differential scanning calorimetry (DSC) together with simultaneous thermal analysis (STA) techniques were used to identify the intermediate phase. 4 7H 2 The dehydration of O takes a certain amount of time, and a high heating rate may shift the dehydration peak to a high temperature, so it is necessary to understand the effect of the heating rate on the dehydration process. To this end, dehydration analysis was performed using DSC under nitrogen at heating rates of 1°C / min, 2°C / min, 5°C / min, and 10°C / min to ensure that oxidation does not occur during the dehydration of Epsom salt.

[0149] Now refer to Figure 4 , showing the MgSO 4 7H 2 O Dehydration heat flow Figure 4 . Table 1 shows a comparison of the heat flow data at these heating rates. The data clearly demonstrate the effect on the dehydration process. The highest heat flow and a more detailed dehydration step were obtained at a heating rate of 5°C / min, a commonly used DSC measurement condition for thermal energy storage materials. The enthalpy measured at this 5°C / min heating rate is also closest to the theoretical enthalpy of pure TCM. Therefore, in further studies, DSC and STA measurements were performed at a heating rate of 5°C / min.

[0150]

[0151] Table 1 shows the effect of heating rate on MgSO 4 7H 2 DSC data of the effect of O dehydration heat flow

[0152] By using MgSO obtained with STA 4 7H 2 O dehydration mass change data and heat flow data from DSC measurements to determine the hydrated intermediate phase (MgSO 4 ·nH 2 O) and heat flow changes.

[0153] Figure 5A It shows that MgSO 4 7H 2 OSTA measurement data 5A at 25℃ to 300℃, Figure 5BDSC data 5B measured at temperatures between 25°C and 150°C are shown, and Figure 5C DSC dehydration data 5C obtained over a temperature range of 25°C to 300°C are shown. MgSO 4 7H 2 The dehydration steps of O are summarized in Table 2.

[0154]

[0155] Table 2 MgSO by STA and DSC 4 7H 2 Dehydration step of O

[0156] In general, MgSO 4 7H 2 The main dehydration step of O occurs after a period of 45 min at 150 °C (see Figure 5A and 5B ), producing MgSO 4 ·H 2 O. This temperature can be achieved fairly easily by heating using, for example, solar collectors, waste heat or renewable / off-peak electricity. MgSO 4 7H 2 The total enthalpy of dehydration of O is about 1376 J / g (using Figure 5A and 5B ), assuming that MgSO 4 7H 2 The density of O is 1.68 g / cm 3 And the sample is heated to 150℃, then 2.30GJ / m 3 The energy density of MgSO is generated after heating to 300 °C in a dry nitrogen atmosphere. 4 7H 2 Complete dehydration of O to give MgSO 4 (See Figure 5A and 5C ). Thermogravimetric analysis (TG) results ( Figure 5A ) showed that when the dehydration temperature was about 150°C, the total mass loss was 40.87%. This is equivalent to a dehydration level of about 80%. When further heated to 300°C, the sample can be completely dehydrated to anhydrous magnesium sulfate. It was found that the measured total mass loss was 50.5% (the theoretical mass loss from magnesium sulfate heptahydrate to anhydrous magnesium sulfate is 51.1%). A small peak was observed at temperatures between 270°C and 275°C, and the mass reached a constant after 275°C. This indicates that 0.2H was lost at 275°C. 2 O to form anhydrous MgSO 4 These results are consistent with XRD analysis ( Figure 3). In conclusion, the combination of XRD, DSC and STA measurements shows that MgSO 4 7H 2 The dehydration of O has seven steps:

[0157] The first step has a mass loss of about 3.23% at 47.7 °C. This corresponds to MgSO 4 7H 2 O dehydrates to MgSO 4 6H 2 O. Note that the theoretical mass loss for this step is 7.3%, the reason for this discrepancy is that the starting material for the reaction was partially dehydrated before the measurement. MgSO 4 7H 2 O to MgSO 4 6H 2 This is supported by the fact that the transformation to O starts at ambient temperature. Therefore, during the storage period of the material before the measurement, about 56.2% of the initial MgSO 4 7H 2 O powder has been dehydrated to MgSO 4 6H 2 O. This is slightly different from the XRD data, in which the initial crystalline phase MgSO was found at 25 °C 4 7H 2 O. This can be explained by the following facts:

[0158] XRD measurements were performed using fresh samples, whereas STA measurements were performed on salt samples after storage for 3 to 6 months.

[0159] The second step has a mass loss of 15.04% at 68.8 °C, producing MgSO 4 ·4H 2 O intermediate phase.

[0160] The third step has a mass loss of about 14.06% at 110 °C, indicating that each mol of MgSO 4 A further loss of 2 mol H 2 O, resulting in a residual water content of 2 mol H 2 O.

[0161] The fourth step occurs at 140.8 °C with a mass loss of 3.17%, corresponding to MgSO 4 1.5H 2 O transition phase.

[0162] The fifth step occurs at 150 °C with a mass loss of 3.48%, resulting in a residual water content of 1 molH 2 O.

[0163] The sixth step occurred between 150°C and 270°C, and 0.8 mol H 2 The mass loss of O.

[0164] The last step yields MgSO at 275 °C with a small mass loss of 1.5% 4 Crystalline phase.

[0165] Example 2 -MgSO 4 Hydration of hydrate

[0166] About MgSO 4 There are few reports on systematic studies of the hydration behavior of hydrates. The key factors affecting the hydration reaction are temperature and humidity. At relative humidity above the equilibrium humidity of the hydration-dehydration reaction, the salt absorbs water to form a higher hydration state. At relative humidity below the deliquescent humidity of the lower hydration state, hydration proceeds as a solid-state reaction, while above the deliquescent humidity, a complete dissolution mechanism occurs. MgSO 4 Hydration of hydrates requires more than 3 hours to reach equilibrium, and some studies have shown that it may take 12 hours to 20 hours, or even up to 100 hours, to reach the final equilibrium. To understand the above, STA, DVS and in situ Raman microscopy were performed.

[0167] Now refer to Figure 6 , showing that about MgSO 4 7H 2 DVS data of the dehydration (desorption) and rehydration (adsorption) processes of O Figure 6 The DVS measurement was performed using the same procedure as the STA measurement, except for the dehydration temperature and hydration time. The dehydration temperature was 135°C, which is the maximum safe operating temperature of the DVS preheating function (limit T < 150°C). The hydration process took 12 hours to ensure that the MgSO 4 The hydrates are allowed sufficient isothermal time to reach equilibrium.

[0168] like Figure 6 As shown, in DVS, MgSO 4 .7H 2 Dehydration of O at 135 °C showed a mass loss of 40% when heated from 25 to 135 °C, which represents 80% of the total water content (corresponding to a mass loss of 50.2% if heated to 150 °C). A similar mass loss was obtained by heating STA to 150 °C. In the subsequent rehydration step, MgSO 4The hydrate reached 80% of the initial mass within 3 hours at 85% RH at 35 °C, and a further 3 hours of hydration reached 92% of the initial mass. The data show that an additional 6 hours were required to reach 97% to 100% of the initial mass. These results indicate that the hydration process requires at least 6 hours. Comparison between the dehydration and hydration data shows that MgSO 4 The hydration (adsorption) process of hydrates is much slower than the dehydration process, about 50% slower.

[0169] Now refer to Figure 7 , showing that MgSO 4 7H 2 Results of the mass change of O after dehydration / rehydration at 25°C, 35°C, 45°C and 55°C Figure 7 The fastest hydration rate was observed at 35 °C, although hydration had not yet reached equilibrium after 6 h. A total mass increase of 37.6% was observed, which represents a maximum water uptake of 86%. Under the same experimental conditions, the MgSO 4 The hydration reaction rate of the hydrate was slower than that measured with the DVS. While not wishing or intending to be bound by any theory, we believe this is because the sample holder of the DVS is a fine mesh disk that allows humid air to flow into the sample from the surrounding environment, while the sample holder of the STA only allows sample-air contact from the top. Figure 7 The observations also showed that the mass loss curves during dehydration were almost identical, while the mass gain curves during hydration depended on the hydration temperature. The data also showed that under the experimental conditions, MgSO 4 The optimal hydration conditions for hydrates were 35 °C and RH 85% for 6 h. 4 Hydrate Phase Figure 1 To.

[0170] Example 3 -MgSO 4 7H 2 Recyclability of O

[0171] It is well known that salt particles change volume, size and morphology during dehydration / hydration cycles. These can have significant effects on heat and mass transfer, leading to reduced kinetics and performance degradation. Little is known about the effects of thermal cycling on MgSO at high cycle times. 4 7H 2 O behavior effects.

[0172] To address the above issues, five thermal cycles were initially performed, which showed that after the first cycle, MgSO 4The rehydration rate of the hydrate increased significantly, and the mass increase of the hydration reaction reached the expected equilibrium value by hydration for 3 hours in the fifth cycle. These initial experiments provided data for setting the thermal cycling conditions for subsequent cycling tests: dehydration for 3 hours, followed by hydration for 3 hours to complete one cycle, followed by a large number of cycles repeated.

[0173] Now refer to Figure 8 , showing 30 cycles of dehydration and hydration Figure 8 During dehydration at 150°C in the first cycle, the heat flow was about 1100 J / g. During rehydration at 35°C and 85% RH in the first cycle, the heat flow was only about 600 J / g, which was only 50% of the dehydration process. Such results were confirmed by TG analysis, which showed a 50% reduction in mass change. In the second cycle, the heat flow of dehydration decreased to about 800 J / k, significantly lower than the first cycle; while the heat flow of hydration increased to about 940 J / g.

[0174] From the second cycle, as the number of cycles increases, a significant increase trend in heat flow and mass change is observed for both dehydration and hydration processes. This trend flattens out after about 10 cycles, where for dehydration, the heat flow increases from about 800 J / g (2nd cycle) to about 1100 J / g (10th cycle), and for hydration, the heat flow increases from about 940 J / g (2nd cycle) to about 1200 J / g (10th cycle). This is supported by TG data. After 10 cycles, the heat flow data between dehydration and hydration reactions are very close, where in the same cycle, the heat flow of hydration is 5% to 10% higher than the heat flow of dehydration, and from the 11th cycle, the mass loss and mass increase are almost the same, which is about 92% of the initial mass loss / mass increase. These results show that under these experimental conditions, MgSO 4 7H 2 O has good cyclability for at least 30 cycles. These observations are encouraging but are derived from small amounts of sample (e.g., 5 mg in DSC and 20 mg in STA).

[0175] To gain a deeper understanding of MgSO 4 7H 2 The cyclability results of O were analyzed at the 1st cycle, 5th cycle, 10th cycle, 20th cycle and 30th cycle, represented by C1, C2, C5, C10, C20 and C30, respectively.

[0176] Now refer to Fig. 9 , showing the MgSO from DSC analysis for different cycles 4 7H 2 Comparison of O dehydration data Fig. 9. Two main peaks appeared during the dehydration process of the first cycle (C1). When the heating temperature was about 45°C, the first peak appeared at 20 minutes and the second peak appeared at 50 minutes. Only one peak (the second peak) was observed in the second and fifth cycles, although these cycles had the same peak profile with a slight shift in the peak position. The peak positions and heat flows of C10, C20, and C30 were significantly different from those of C5, C2, and C1, but the peak positions of C10, C20, and C30 were the same.

[0177] By using SEM to characterize the morphology of materials subjected to thermal cycling, and Fig.10 A to 10D show MgSO 4 7H 2 Results of O samples before and after dehydration at 150 °C and hydration at 35 °C and 85% RH in STA, where Fig.10 A is before the first cycle starts, Fig.10 B is after one cycle, Fig.10 C is after five cycles, and Fig.10 D is after 30 cycles.

[0178] Fig.10 A shows the MgSO 4 7H 2 SEM image of the crystalline morphology of O 10, where the particle size is about 0.2 mm to 0.5 mm, and there are fine cracks 11 distributed over the entire sample surface. After the first cycle, the volume of the particle 10' is slightly larger than that of the raw material 10 ( Fig.10 B compared to Fig.10 A), and some coarse cracks 11' were observed on the entire sample surface, indicating that the salt particles expanded during the cycles. These indicate that after the first cycle, fine cracks were generated in the crystals 10', forming a form that more easily releases water molecules. This could explain why the hydration heat flow increased significantly starting from the second cycle. Fig.10 C shows that after the 5th cycle, the particle 10" appears to swell and form large cracks, creating some air / water flow paths 11". Fig.10 The enlarged image of the particle 10" in C shows that the particle is an agglomerate of small crystals. Fig.10 As shown in Figure D, a different morphology is observed after 30 cycles. The size of the particles 10"' becomes larger (>0.5 mm) and the air / water flow channels 11"' are much larger. These morphological and dimensional changes during thermal cycling can explain, at least in a qualitative way, the increase in reaction enthalpy in the first 3 to 5 cycles, during which cracks are generated and thus more air / water flow channels and / or reaction surface area are created.

[0179] Note that Fig.10The significant change in the morphology of the salt particles, as shown in D, seems to indicate structural stability of the pure salt. Such changes have little effect on the heat of reaction within 30 cycles, mainly because the sample amount is small (e.g., 5 mg in DSC or 20 mg in STA), so no significant heat and mass transfer effects are expected. Given the significant morphological changes and the resulting structural changes, an increase in sample amount may affect the kinetics due to heat and mass transfer. To date, the progress in the MgSO 4 7H 2 There has been little progress in the practical application of O to prove this.

[0180] Example 4 - MgSO in different preparations 4 7H 2 Hydration / dehydration of O composites

[0181] In order to determine the optimal composite formulation, two types of composites (MgSO 4 7H 2 O / MgO and MgSO 4 7H 2 O / vermiculite) were subjected to DSC measurement.

[0182] Preparation of MgSO with different percentages using MgO or vermiculite as the host material 4 7H 2 O salt composites, forming two series of MgSO 4 7H 2 O composite samples. These samples were cycled in a high temperature humidity chamber and analyzed with DVS. Each measurement was repeated three times.

[0183] Example 4A

[0184] · 10 wt%, 20 wt%, 30 wt%, 40 wt%, 50 wt% and 60 wt% MgSO prepared with 0.25 mm MgO or vermiculite 4 7H 2 OMgSO 4 7H 2 Heat flow of O composites before and after one dehydration / hydration cycle ( Fig.11 ).

[0185] Example 4B

[0186] 60 wt% MgSO prepared with different vermiculites of particle sizes 0.08 mm, 0.125 mm, 0.25 mm, 0.5 mm and 1 mm 4 7H 2 O / Vermiculite composites( Fig.12 ).

[0187] Example 4C

[0188] · MgSO containing 50 wt% and 60 wt% prepared with different vermiculite particles with particle sizes of 0.08 mm, 0.125 mm, 0.5 mm and 1 mm 4 7H 2 MgSO in the form of compacted pellets / modules and non-compacted powder 4 7H 2 O / Vermiculite composites( Fig.13 ).

[0189] The surface analysis data of the host materials determined by mercury porosimetry and nitrogen physisorption BET are summarized in Table 3. The total porosity (Φ), bulk density (P 堆积 ) and median pore diameter (D m The BET data listed are for an upper pore size limit of 13 nm, including the median diameter (D 13 ), total surface area (SSA) and total porosity (Φ 13 Specific pore volume (V p ) Based on the total porosity and density data, V p =(Φ+Φ 13 ) / P 堆积 calculate.

[0190]

[0191] Table 3 Mercury intrusion porosimetry (Φ, P 堆积 , D m ) and nitrogen physical adsorption (D 13m , SSA, Φ 13 ) obtained from the main material data.

[0192] The contribution of small pores with a median pore size of about 6.8 nm in 1 mm vermiculite is considerable (Φ 13 =6.7%). The same is true for MgO particles. Small pores with a median pore size range of 7.52nm to 8.58nm are also present in vermiculite with other particle sizes, but the contribution of small pores to the total porosity of these particle sizes is small. The bulk density and surface area of ​​vermiculite increase with decreasing particle size, while the total porosity, specific pore volume and D m Both decrease with the decrease of particle size.

[0193] Example 4A – Single cycle hydration / dehydration

[0194] Now refer to Fig.11, showing the original MgSO 4 7H 2 O / vermiculite and MgSO 4 7H 2 DSC results of dehydration heat flow of O / MgO composites (i.e. before the first cycle) and after one dehydration / hydration cycle Fig.11 .

[0195] It can be seen that the heat flow increases with the MgSO 4 7H 2 The O percentage increases significantly with the increase in the 4 7H 2 O compositions have a heat flow of over 600 J / g. Containing 60% MgSO 4 7H 2 The dehydration heat flux of the composites with O ranges from 658 J / g to 749 J / g. Fig.11 It is also shown that the two series of MgSO 4 7H 2 The O composites were stable after one cycle, and the cycled composites produced approximately 10% to 30% higher heat flow compared to the heat flow of the uncycled samples.

[0196] Example 4B – Effect of vermiculite size

[0197] Now refer to Fig.12 , showing the relationship between the particle size of vermiculite and MgSO 4 7H 2 Effect of dehydration on O / vermiculite composites Fig.12 .

[0198] DSC results show that the 60% MgSO 4 7H 2 The dehydration heat flux of the composites of MgSO4 ranged from 658 J / g to 758 J / g, where the vermiculite particle size varied from 0.08 mm to 1 mm (the thermal enthalpy of raw vermiculite is about 150 J / g). These data indicate that the particle size of vermiculite has an important effect on the dehydration heat flux of MgSO4. 4 7H 2 The effect of dehydration on the O composites is relatively small, although the heat flow appears to be slightly higher when the particle size of the vermiculite is between 0.5 mm and 1 mm.

[0199] Example 4C —Compound MgSO 4 7H 2 Effect of O-hydrate form

[0200] Now refer to Fig.13, showing MgSO in compacted pellet form and powder form 4 7H 2 Dehydration heat flow of O / vermiculite composites Fig.13 The composite in pellet form is dense and expected to have a higher effective thermal conductivity, but interparticle mass transfer may be affected, while the composite in powder form has a lower effective thermal conductivity, but mass transfer is less restricted. This suggests that the enthalpy difference between the two forms of composites may be small under the conditions of this set of experiments due to the balance between heat and mass transfer effects, which is indeed reflected by Fig.13 The data shown is reflected.

[0201] Although the pellets contained 50% and 60% MgSO during dehydration 4 7H 2 The heat flow data of the composites of MgSO4 and MgSO4 in powder form have small differences, but the heat flow data of the composites in pellet form are 4 7H 2 The O composites showed no or almost no variation between the three repeated measurements and were therefore considered to be more stable than their counterparts in powder form.

[0202] Example 5 -MgSO 4 Hydration / dehydration of hydrate composites

[0203] For MgSO containing 60% salt hydrate 4 7H 2 O / MgO and MgSO 4 7H 2 O / vermiculite composites were subjected to DVS measurements. For comparison purposes, pure MgSO 4 7H 2 The same DVS procedure was performed for both dehydration and hydration. The results are shown in Fig.14 and Fig.15 middle.

[0204] Now refer to Fig.14 , showing the MgSO measured by DVS 4 7H 2 Dehydration (desorption) and hydration (adsorption) data of O / MgO composites Fig.14 When heated from 25°C to 135°C, 60 wt% MgSO 4 7H 2 The O / MgO composite pellets produced a 23% mass loss, which was 76% of the total water content (30.2% total in hydrate). 4The hydration of the hydrated composites was carried out at 85% RH at 35 °C and the hydration process lasted for 2 h to reach 100% of the initial mass. These data are comparable to those of pure MgSO 4 Hydrate data ( Figure 6 ) show that the use of the host material significantly increases the hydration reaction rate.

[0205] Now refer to Fig.15 , showing that MgSO 4 7H 2 DVS dehydration (desorption) and hydration (adsorption) data of O / vermiculite (0.25 mm) composites Fig.15 MgSO 4 7H 2 O / MgO composites Fig.14 Similar observations are shown.

[0206] Now refer to Fig.16 , showing a comparison of MgSO with different vermiculite particle sizes 4 7H 2 DVS dehydration and hydration data of O composites within two cycles Fig.16 .and Fig.12 The data shown are consistent, with only small differences seen in the rehydration kinetics.

[0207] The above results indicate that MgO and vermiculite not only provide a structure to accommodate salt hydrates, but also accelerate the rehydration process (about 2 h, relative to pure MgSO 4 7H 2 O for 6 to 12 hours) and significantly improved the adsorption kinetics. In order to ensure that MgSO 4 The hydrated composites were allowed sufficient isothermal time to reach equilibrium, and a 3 h hydration time was used in subsequent experiments on the composites.

[0208] Example 6 -MgSO 4 7H 2 O Recyclability of composite materials

[0209] MgSO containing 60% salt hydrate 4 7H 2 O / MgO and MgSO 4 7H 2O / vermiculite composites both show promising results in terms of energy density and rehydration kinetics. These data are for a single dehydration-hydration cycle or a limited number of cycles (up to 5 cycles). The multi-cycle stability of composites is critical for practical applications. To understand this, 35 dehydration / hydration cycles were performed and the effects of thermal properties during the cycles were analyzed.

[0210] Example 6A –MgSO 4 7H 2 Recyclability of O / MgO composites

[0211] Now refer to Fig.17 , showing that providing 60 wt% MgSO 4 7H 2 O / MgO cycle results Fig.17 . The heat of reaction measured for the 60% salt in the first cycle was 500 J / g. After three cycles, the heat of reaction increased slightly to about 550 J / g. Starting from the 4th cycle, there was a significant downward trend in heat flow in both the dehydration and hydration processes as the number of cycles increased. This trend became flat after 16 cycles, where the heat flow stabilized at about 250 J / g (about 50% of the first cycle). This is also reflected and consistent with the reduction in mass change from 100% to 50%. No further reduction in heat flow and mass change was observed after the 17th cycle. These results show that in terms of energy density, 60 wt% MgSO 4 7H 2 The O / MgO composite decreases in the first 16 cycles but then stabilizes at an energy density of about 250 J / g. Although not ideal for long-term energy storage, this energy density is still highly competitive with sensible and latent heat storage, considering that there is only 60% salt in the composite. Given the low cost of the raw materials, this still has good potential for short- and medium-term energy storage applications.

[0212] Example 6B – Recyclability of vermiculite composites

[0213] Fig.18 It is shown that 60 wt% MgSO 4 7H 2 Cycle results of O / 0.5 mm vermiculite composites Fig.18 .

[0214] The figure shows that MgSO 4Excellent cyclability of the MgSO / vermiculite composite over 35 cycles, with hydration heat flows ranging from 612 J / g to 827 J / g and dehydration heat flows ranging from 639 J / g to 774 J / g. The mass changes during hydration and dehydration vary within a small range, consistent with the changes in hydration / dehydration heat flows. Note that the data are for a 60% salt loading in the composite. If the adsorption heat of vermiculite is taken as 150 kJ / kg, the contribution of the host material to the total adsorption heat is 60 kJ / kg, and the MgSO 4 The contribution of salt is 690 kJ / kg, which is equivalent to pure MgSO 4 1150kJ / kg of salt.

[0215] Then MgSO 4 7H 2 DSC analysis was performed on the 1st, 10th, 20th, 30th and 35th cycles (C1, C10, C20, C30 and C35) of O / vermiculite dehydration / hydration. Fig.19 The results show that 60 wt% MgSO 4 7H 2 Comparison of C1, C10, C20, C30 and C35 cycles of O / 0.5 mm vermiculite composites Fig.19 For each of the cycles (C1, C10, C20, C30, and C35), the same thermal enthalpy curves were obtained in both the dehydration and hydration processes, indicating the excellent stability of the composite materials.

[0216] Fig. 20 shows 60 wt% MgSO 4 7H 2 O / MgO( Fig. 20 A) and 60 wt% MgSO 4 7H 2 O / Vermiculite( Fig. 20 B) Images before and after STA cycle testing. These images show macroscopically that the two MgSO 4 7H 2 The O composite remained structurally stable after 35 cycles of dehydration and hydration, although the surface morphology changed.

[0217] Fig.21 A to 21E show the original MgO 210, the original MgSO 4 7H 2 O 211, original MgSO 4 7H 2 O / MgO composite material 212, and MgSO after five cycles 4 7H 2O / MgO composites 212' and MgSO after 35 cycles 4 7H 2 Microscopic SEM image of a sample of O / MgO composite 212".

[0218] Fig.21 A shows agglomerated submicron / nano-sized spherical MgO particles 210 with a diameter of 0.5 μm to 0.7 μm and an agglomerate size of 5 μm to 10 μm. Fig.21 B shows MgSO 4 7H 2 The morphology of O 211, which can have a crystal size of about 0.2 mm to 0.5 mm and fine cracks 213 distributed across the sample surface. Fig.21 C shows spherical MgO and MgSO that are ground into smaller particles than MgO agglomerates and contain submicron / nano sized particles. 4 7H 2 O morphology of the composite material 212. Fig.21 D shows a composite sample 212" formed with cracks and channels 214 for air / moisture gas flow. Fig.21 E shows that the composite sample 212" shows a completely different and interesting morphology. The morphology shows egg-shaped units with a diameter of 1 μm to 3 μm, and fine cracks 214' on the entire surface of the egg-shaped units, which can be used to stabilize the heat flow after the 16th cycle ( Fig.17 ) provide an explanation. These results seem to indicate that the salt particles are mainly in the intergranular spaces of the thermochemical material.

[0219] Fig. 22 The SEM images shown in A to 22D are respectively vermiculite 220, raw MgSO 4 7H 2 Samples of O / 60% / vermiculite composite 221, composite 221' after three cycles, and composite 221" after 35 cycles.

[0220] The raw vermiculite sample 220 (0.5 mm particle size) consisted of layers in the form of stacked sheets ( Fig. 22 A). Fig. 22 B shows the morphology of the composite material 221 having fine cracks 222 on the surface of the sample. Fig. 22 C shows that the composite sample 221 ′ has become more porous, with cracks, making the structure less resistant to absorbing and releasing water than the original structure because more surface area and channels are available. Fig. 22D shows a composite sample 221" having a more highly porous morphology with a loosely agglomerated network containing macropores and channels 223 for air / moisture, with pore diameters ranging from 2 μm to 10 μm. These results appear to indicate the presence of salt in both inter-particle and intra-particle voids.

[0221] Example 7 –MgSO 4 7H 2 O / Vermiculite composite modules / pellets circulation in humidity chamber

[0222] It has been shown that MgSO 4 7H 2 The O / vermiculite composites have excellent recyclability within 35 cycles ( Fig.18 , Fig.19 ). These cycling tests were performed in a STA instrument under well-controlled conditions with very small samples (about 20 mg). It would be useful to know whether the conclusions also hold true for larger samples made under different compaction conditions and subjected to a greater number of cycles in a less well-controlled environment.

[0223] To this end, the preparation of composite compacted pellets at different compaction pressures of 10 MPa, 20 MPa, 30 MPa and 40 MPa was first studied. A loading speed of 20 mm / min was used for compression with a holding time of 1 minute before unloading. The diameter of the composite pellets was 13 mm and each had a mass of 1.5 g. The pellets were then placed in a high temperature humidity chamber and cycled 100 times under conditions similar to those in the STA. The composite pellets were then characterized after different numbers of cycles.

[0224] Fig.23 A to 23D show 60 wt% MgSO 4 7H 2 Images of O / 0.5 mm vermiculite pellets after 0 cycles, 10 cycles, 30 cycles, and 100 cycles, where sample 230 was prepared at 10 MPa, sample 231 was prepared at 20 MPa, sample 232 was prepared at 30 MPa, and sample 233 was prepared at 40 MPa.

[0225] As the number of thermal cycles increases, changes in pellet morphology and integrity are evident. After 10 cycles, the pellets are seen to swell slightly ( Fig.23 B), after 30 cycles the structure of the pellets appears loose and fragile, with some powder falling off from the original structure ( Fig.23 C), after 100 cycles, most of the pellets became powdery and the structure became weak, losing the original pellet shape / structure ( Fig.23 D).

[0226] XRT analysis was performed on samples that were cycled 30 times, where the samples were made at different compaction pressures (10 MPa, 20 MPa, 30 MPa, and 40 MPa) to study the morphology and changes in the pellet structure. The results are shown in Fig.24 A to 24C, among which Fig.24 A is original 60 wt% MgSO at 10 MPa, 20 MPa, 30 MPa and 40 MPa 4 7H 2 2D image of O / vermiculite composite pellets, Fig.24 B is the 2D image of the composite material under 10MPa, 20MPa, 30MPa and 40MPa after 30 cycles, Fig.24 C is the 3D image of the composite material at 10 MPa, 20 MPa, 30 MPa and 40 MPa after 30 cycles.

[0227] like Fig.24 The dark areas 240 in the 2D image of the original composite material are pores or air paths as shown in A. Smaller pores and fewer air paths are observed at higher compaction pressures. Fig.24 B shows that the porous structure of the cycled samples has cracks 241 formed between the outer and inner layers of the pellet. The pellets at 40 MPa have the largest cracks and have lost their original circular shape. 3D images of these cycled samples ( Fig.24 C) shows that the pellets at 20 MPa maintained a relatively round shape compared to the pellets at other compaction pressures. Overall, all the recycled pellets developed cracks.

[0228] The pellet expands and cracks starting from the top, where contact with air / moisture occurs faster and easier than in other parts of the pellet.

[0229] Ring cracks can be related to the loading / unloading speeds during manufacturing. To understand these effects, the loading speed was reduced from 20 mm / min to 10 mm / min and the holding time was increased from 1 min to 3 min. The compression pressures studied were 15 MPa, 20 MPa, 25 MPa and 30 MPa. Fig.25 Images of the original pellet 250 prepared using the new process, as well as pellets 251 after 16 cycles and pellets 252 after 30 cycles are shown. XRT analysis was also performed on the original pellets and the pellets after 30 cycles in the humidity chamber, and the results are shown in Fig.26 A and 26B.

[0230] like Fig.25As shown in Figure 2, pellets (250, 251, and 252) prepared using the new manufacturing process show significantly better structural integrity than pellets prepared at higher loading rates and shorter holding times. For pellets cycled 30 times, although cracks can be observed from the surface, the structural integrity is maintained. This is also supported by XRT analysis, such as Fig.26 A and Fig.26 As shown in B.

[0231] Fig.26 A shows the original 60 wt% MgSO prepared using the new process described above at compression pressures of 15 MPa, 20 MPa, 25 MPa, and 30 MPa. 4 7H 2 2D images of O / vermiculite pellets. They resemble Fig.24 2D image of the original pellet is shown in .

[0232] Fig.26 B shows a 2D image of a pellet that has undergone 30 cycles. As shown, four sets of images were taken from pellets prepared with different pressures. Each set of images includes a 3D image of a cylindrical pellet (center left) and three 2D images taken from three cross-sections of the cylindrical pellet at different vertical positions (upper image from the top of the pellet; center right image from the middle of the pellet; and lower image from the bottom of the pellet). For all pellets, it is seen that cracks 260 have formed between the outer and inner layers of the cylindrical wall, and cracks at the top of the pellet may be due to easy contact with air / water vapor. Small cracks are also seen in the middle and bottom of the pellet. These images also show that despite the formation of cracks, structural integrity is maintained within 30 cycles.

[0233] XRD analysis at ambient conditions was also performed to investigate the chemical stability and compatibility of the composites subjected to different cycles, while DSC measurements were performed on the composites to understand the effect of thermal cycling on the reaction enthalpy. The results are shown in Fig. 27 and Fig.28 middle.

[0234] Fig. 27 shows 60 wt% MgSO 4 7H 2 XRD results of O / vermiculite pellets after 0 cycles (original), 10 cycles, 30 cycles, 40 cycles, 60 cycles, 80 cycles and 100 cycles in the humidity chamber Fig. 27 In all cycles, the samples obtained the same crystalline phase, indicating that after 100 cycles, MgSO 4 7H 2 The crystallinity and phase of O / vermiculite composites did not change, indicating the excellent chemical stability and component compatibility of the composites.

[0235] Fig.28 shows 60 wt% MgSO 4 7H 2 DSC results of O / vermiculite pellets after 0 cycles (original), 10 cycles, 30 cycles, 40 cycles, 50 cycles, 80 cycles and 100 cycles Fig.28 Although the heat flow measured by DSC fluctuated in different cycles, no obvious decrease was observed, indicating very good cyclability.

[0236] Example 8 – Addition of binder

[0237] In order to further enhance the structural integrity and mechanical strength of the composite material, the addition of a small amount of binder was studied. In this study, as described in Example 7, a lower compression speed was used to prepare pellets with a longer pressure holding time. The water-soluble polymer polyvinyl pyrrolidone (polyvinylpyrrolidone PVP) was selected due to the good adhesive properties, high melting temperature (≥150°C) and hygroscopic properties of PVP. The aqueous solution of PVP (H 2 The effect of PVP concentrations of 0.5 wt%, 1 wt%, 2 wt% and 3 wt% relative to the weight of the composite (i.e., the weight % of PVP in the proportion of TCM) was studied. The pellets were placed in a high temperature humidity chamber and cycled 80 times. Fig.29 Photos of the pellets after 0 cycles (original), 20 cycles, 40 cycles and 80 cycles are shown. After 20 cycles, almost no changes can be seen in the pellets with different binder concentrations. Slight expansion of the pellets is seen after 40 cycles, and further expansion occurs after 80 cycles but the structural integrity is still high. Observation of these photos shows that the pellets with 20 MPa and 2% binder concentration give the best structural integrity.

[0238] MgSO with 2 wt% binder 4 7H 2 The O / vermiculite composite pellets were subjected to DSC analysis to understand whether the use of a binder affects the dehydration and hydration kinetics. Fig.30 60 wt% MgSO with 2% binder (PVP) is shown. 4 7H 2 Heat of reaction of O / vermiculite composites as a function of cycle number Fig.30 MgSO with 2% binder 4 The good recyclability of the / vermiculite composite material can be seen within 30 cycles, Fig.29The heat flow is consistent with the observations shown. Over 30 cycles, the heat flow is seen to be about 900 ± 200 J / g, consistent with the mass change. Note that this data is for a composite with 39.2% host material and 2% binder with 58.8% salt loading. If the heat of adsorption of vermiculite is taken as 150 kJ / kg, the host material contributes 58.8 kJ / kg to the total heat of adsorption, and MgSO 4 The contribution of salt is about 840 kJ / kg, which is very close to pure MgSO 4 Theoretical energy density of salt.

[0239] The results detailed above demonstrate the distinct advantages of the composite TCM pellets, including high energy density, high chemical stability and compatibility, good reaction kinetics, a high degree of structural integrity, and high cyclability.

[0240] Although the above data prove the effect of hydrated magnesium sulfate, other potential CTMs can also be used instead of it. In addition, the host material need not be limited to vermiculite and MgO, but can be other inorganic substances. In addition, the binder need not be limited to PVP, but can be other binders, such as starch, alginate, casein, cellulose binders such as hydroxypropyl methylcellulose (HPMC), polyvinyl acetate (PVA), polyacrylic acid, etc.

[0241] Furthermore, although the above description relates to a compaction manufacturing process, the TCM may also be manufactured using, for example, a pelletizing or extrusion process.

[0242] The present invention will now be further described, by way of example only, with reference to the accompanying drawings, in which:

[0243] Fig.31 A flow chart showing a batch process for manufacturing a composite thermochemical material in pellet form;

[0244] Fig.32 A flow chart showing a continuous process for manufacturing a composite thermochemical material in extruded form;

[0245] Fig.33 A graph showing a comparison of the measured reaction enthalpies of composite TCMs made by pelletizing and extrusion;

[0246] Fig.34 Provides images showing the shape stability of granular composite TCM and extruded composite TCM;

[0247] Fig.35 Provides images showing the structure of composite TCM in pellet form;

[0248] Fig.36 provides images showing the structure of a composite TCM in extruded form; and

[0249] Fig.37 Figure 2 is a graph of the dehydration / hydration of extruded samples after different thermal cycles.

[0250] Now refer to Fig.31 , showing the use of forming a deliquescent material (e.g., SrBr 2 6H 2 O) and non-deliquescent materials (e.g. MgSO 4 7H 2 O) Exemplary process of granular TCM of both.

[0251] In each case, the first step or stage 31A comprises grinding the subject material (e.g., vermiculite or MgO) to an optimal size range (e.g., 0.08 mm to 1 mm) and mixing the subject material with up to 80% by weight, e.g., 20% to 80% by weight, for example, 40% to 70% by weight of salt hydrate. In one embodiment, 60% by weight of salt hydrate is used.

[0252] In the second step or stage 31Bi of the deliquescent material, mixing can be carried out under deliquescent conditions (i.e., at a relative humidity sufficient to deliquesce the material) so that the TCM can diffuse into the inter-particle and intra-particle voids of the host material. The resulting mixture is fed to the third step 3 or stage. If the mixture has poor flowability, a drying step can be employed to increase the flowability of the mixture, and flow aids can also be added in this stage.

[0253] In a second step or stage 31Bii of the non-deliquescent material, the salt hydrate is ground to micron size, e.g., 1 μm to 100 μm, while mixing the salt hydrate with the host material in a media mill, e.g., a ball mill, wherein the grinding ball size is 200 μm to 100 μm. http: / / www.minproc.pwr.wroc.pl / journal / pdf / ppmp48-2.329-339.pdf. This stage may also include the addition of flow aids.

[0254] In both cases, the third step or stage 31C can include mixing the material from the second stage with up to 5% by weight of a binder (e.g., a binder selected from polyvinyl pyrrolidone (PVP), starch, alginate, casein, a cellulose binder such as hydroxypropyl methylcellulose (HPMC), polyvinyl acetate (PVA), polyacrylic acid, and mixtures thereof. The binder is present as a solution.

[0255] In a fourth step or stage 31D, the material mixture from stage 31C is granulated using a high shear mixer (e.g., a Cyclomix (RTM) high shear mixer available from Hosokawa Micron BV, Doetinchem, The Netherlands). Granulation conditions are such that dense granules are formed, preferably substantially round granules of, say, 2 mm to 8 mm in size. Under exemplary conditions (room temperature, 2% binder addition), deliquescent materials can be formed into granules of 5 mm to 8 mm in size (as shown in 31Di), and non-deliquescent materials can be formed into granules of 2 mm to 5 mm in size (as shown in 31Dii).

[0256] Now refer to Fig.32 , showing an exemplary process for forming an extruded composite TCM.

[0257] In a first step or stage 32A, the subject material is ground in the same manner as described above at 31A.

[0258] In a second step or stage 32B, the salt hydrate is ground to micron size, for example 1 μm to 100 μm, while mixing it with the host material in a grinder, such as a ball mill, in the same manner as in 31Bi or 31Bii.

[0259] In a third step or stage 32C, a binder (eg, up to 5 wt. % binder) is added to the ground mixture from the second stage 32B and the mixed material is then extruded.

[0260] The material is extruded through a die (a thick steel disk with an opening) to form a composite TCM, for example, with an outer diameter of 2 mm to 20 mm for this type of application. As shown in 32D, the extruded TCM is MgSO with a 5 wt% PVP binder and an outer diameter of about 4 mm. 4 7H 2 O / MgO (60 wt% / 35 wt%).

[0261] Reference Fig.33 The granular composite TCM (33A) and the extruded composite TCM (33B), each comprising MgSO with 5 wt % PVP binder, were subjected to STA as described in detail in Section 3 (Material Characterization) above. 4 7H 2 The reaction enthalpy (energy density) of O / MgO (60 wt% / 35 wt%) was evaluated.

[0262] Fig.33 The energy densities shown in the figure are 812 J / g and 783 J / g, respectively, which is equivalent to 0.92 GJ / m 3 or 255kWh / m3 (granular composite TCM) and 0.89GJ / m 3 or 246kWh / m 3 (Extruded composite TCM), demonstrating the feasibility of fabricating composite TCM using the two methods.

[0263] As will be appreciated, extrusion routes may be particularly beneficial because continuous process routes can generally exhibit production advantages over batch processes.

[0264] The present invention will be further described with reference to the following examples.

[0265] Example 9A – Thermal Cycle of Granular Composite TCM

[0266] In with Fig.30 Under the same conditions, the above process ( Fig.31 ) prepared granular composite MgSO 4 / Vermiculite TCM subjected to thermal cycling.

[0267] Fig.34 Granular materials at 0 cycles (34Ai), 30 cycles (34Bi), and 80 cycles (34Ci) are shown. The size of the granular composite TCM was observed to increase up to 30 cycles and then remained essentially constant in subsequent cycles, indicating good structural integrity of the composite material.

[0268] Fig.35 A comparison between TCM granules at 0 cycles (lower image) and 80 cycles (upper image) is shown. At 0 cycles, the nominal size of the granules was 5 mm, while at 80 cycles, it increased to 7 mm (a 40% increase in size or about 275% increase in volume). However, 2D and 3D images taken using SEM and XRT techniques, respectively, showed little evidence of cracking or structural weakness, supporting the structural integrity of the granular composite TCM after 80 cycles.

[0269] Example 9B – Thermal Cycle of Extrusion TCM

[0270] Fig.36 A comparison between extruded TCM at 0 cycles (lower graph) and 13 cycles (upper graph) is shown. At 0 cycles, the nominal size of the extrudate was 3.7 mm, while at 13 cycles it increased to 3.8 mm (a 3% increase in size). By comparison Fig.34 Aii, Fig.34 Bii and Fig.34Cii demonstrates that the size / volume change after 80 cycles is still small. 2D (SEM) and 3D (XRT) images show little evidence of cracking or structural weakness, indicating the structural integrity of the extrudate.

[0271] Reference Fig.37 , showing 60 wt% MgSO with 5% binder (PVP) 4 7H 2 DSC measurement results of the heat of reaction of the extrudates of the O / vermiculite / MgO composites as a function of the number of cycles. Good cyclability of the extrudates over 13 cycles can be seen. The heat flow over 13 cycles is seen to vary from about 800 ± 200 J / g, consistent with the mass change of the thermal cycles.

[0272] The above results show that the hydrated or hydratable salt material provided in the formed TCM in a proportion of more than 40% by weight, preferably more than 50% by weight, for example more than 55% by weight has the desired mechanical stability and thermal cycling performance. The hydrated or hydratable salt material is found in the intergranular voids of the inorganic host material and in the porous structure. In more porous or plate-like or layered host materials such as vermiculite, the proportion of hydrated or hydratable salt material in the intragranular voids may be higher than that of materials with fewer pores such as MgO. Providing a binder, such as 2% by weight of a binder, can help to consolidate the TCM without compromising performance.

[0273] The results detailed above clearly demonstrate the advantages of the composite TCMs prepared by pelletization, tableting, extrusion, and granulation, including high energy density, high chemical stability and compatibility, good reaction kinetics, high degree of structural integrity, and high cyclability.

Claims

1. A method of forming a composite thermochemical material, the method comprising providing an inorganic host material and providing a hydrated or hydratable inorganic salt, mixing the inorganic host material and the hydrated or hydratable inorganic salt to form a mixture, allowing or causing at least a portion of the hydrated or hydratable inorganic salt to enter the pores and / or void spaces of the inorganic host material, and forming the mixture into a shaped body.

2. A method according to claim 1, comprising providing the inorganic host material as particles.

3. The method according to claim 1 or 2 comprises providing the inorganic host material in a size range of 0.01 mm to 10 mm, for example, from any one of 0.02 mm, 0.03 mm, 0.4 mm or 0.05 mm to any one of 10.0 mm, 9.0 mm, 8.0 mm, 7.0 mm, 6.0 mm, 5.0 mm, 4.0 mm, 3.0 mm, 2.0 mm, 1.0 mm.

4. A method according to any one of claims 1, 2 or 3, comprising providing the hydrated or hydratable inorganic salt as particles.

5. A method according to any preceding claim, comprising providing the hydrated or hydratable inorganic salt in or having a size range of 0.01 μm to 100 μm.

6. A method according to any preceding claim, comprising providing the hydrated or hydratable inorganic salt in a weight ratio of 20 wt% to 80 wt% and / or providing the inorganic host material in a weight ratio of 80 wt% to 20 wt%, preferably providing more than (wt%) of the hydrated or hydratable salt of the inorganic host material.

7. A method according to any preceding claim, comprising providing more of the hydrated or hydratable salt by mass than the inorganic host material.

8. A method according to any preceding claim, comprising providing a binder.

9. A method according to any preceding claim, comprising providing a binder to the mixture, and preferably subsequently mixing.

10. A method according to any preceding claim comprising providing the binder in an amount of up to 5 wt%.

11. A method according to any preceding claim, wherein the mixing, preferably under shear, causes or allows at least a portion of the hydrated or hydratable inorganic salt to enter the pores of the inorganic host material.

12. A method according to any preceding claim, comprising adding a flow aid, for example up to 5 wt %.

13. The method according to any one of claims 1 to 10, comprising exposing the mixture to relatively high humidity conditions, which provide a deliquescent environment for the hydrated or hydratable inorganic salt to enable or allow at least a portion of the hydrated or hydratable inorganic salt to enter the pores of the inorganic host material.

14. A method according to any preceding claim, comprising forming the mixture into a shaped body by one or more of pelletising, tabletting, granulating or extruding the mixture.

15. A method according to any preceding claim, comprising providing the shaped body with a maximum transverse dimension in the range 1 mm to 600 mm.

16. A composite thermochemical material comprising a mixture of particles of a hydrated or hydratable inorganic salt and an inorganic host material, wherein at least a portion of the hydrated or hydratable salt is located within the pores and / or void spaces of the inorganic host material, and the hydrated or hydratable salt is present in an amount greater than 40 weight percent.

17. A composite thermochemical material according to claim 16, wherein the hydrated or hydratable inorganic salt is selected from MgSO4·7H2O, K2CO3·H2O, CaSO4·2H2O or SrBr2·6H2O, Al2(SO4)3·6H2O, CuSO4·5H2O, Li2SO4·H2O, Ca(OH)2, Mg(OH)2·H2O, Fe(OH)2, Na2S·5H2O, CaCl2·6H2O, MgCl2·6H2O or a mixture thereof.

18. The composite thermochemical material according to claim 16 or 17, wherein the theoretical volume energy density of the hydrated or hydratable inorganic salt is 1.0 GJ / m 3 , 1.1GJ / m 3 , 1.2GJ / m 3 , 1.3GJ / m 3 , 1.4GJ / m 3 , 1.5GJ / m 3 , 1.6GJ / m 3 , 1.7GJ / m 3 , 1.8GJ / m 3 , 1.9GJ / m 3 , 2.0GJ / m 3 , 2.1GJ / m 3 , 2.2GJ / m 3 , 2.3GJ / m 3 , 2.4GJ / m 3 , 2.5GJ / m 3 , 2.6GJ / m 3 , 2.7GJ / m 3, 2.8GJ / m 3 , 2.9GJ / m 3 、3.0GJ / m 3 、3.1GJ / m 3 or 3.2GJ / m 3 , or higher than 1.0GJ / m 3 , 1.1GJ / m 3 , 1.2GJ / m 3 , 1.3GJ / m 3 , 1.4GJ / m 3 , 1.5GJ / m 3 , 1.6GJ / m 3 , 1.7GJ / m 3 , 1.8GJ / m 3 , 1.9GJ / m 3 , 2.0GJ / m 3 , 2.1GJ / m 3 , 2.2GJ / m 3 , 2.3GJ / m 3 , 2.4GJ / m 3 , 2.5GJ / m 3 , 2.6GJ / m 3 , 2.7GJ / m 3 , 2.8GJ / m 3 , 2.9GJ / m 3 、3.0GJ / m 3 、3.1GJ / m 3 or 3.2GJ / m 3 .

19. A composite thermochemical material according to any one of claims 16, 17 or 18, wherein the hydrated or hydratable inorganic salt is present in a percentage higher than 45 wt%, for example higher than 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt% or 80 wt%, and / or wherein the inorganic host material is present in a percentage lower than 60 wt%, for example lower than 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt%, 20 wt%.

20. The composite thermochemical material according to any one of claims 16 to 19, wherein the inorganic host material is selected from vermiculite, zeolite, MgO, diatomaceous earth, clay, silica gel, porous glass, attapulgite, graphite, activated carbon, graphite and / or combinations thereof.

21. A composite thermochemical material according to any one of claims 16 to 21, wherein the diameter of the particles of the inorganic host material exceeds 0.02 mm, for example in the size range of 0.02 mm, 0.03 mm, 0.4 mm or 0.05 mm to 10.0 mm, 9.0 mm, 8.0 mm, 7.0 mm, 6.0 mm, 5.0 mm, 4.0 mm, 3.0 mm, 2.0 mm, 1.0 mm, preferably in the range of 0.05 mm to 1 mm.

22. The composite thermochemical material according to any one of claims 16 to 22, further comprising a binder, and wherein the binder can be selected from polyvinyl pyrrolidone (povidone PVP), starch, alginate, casein, cellulose binders such as hydroxypropyl methylcellulose (HPMC), polyvinyl acetate (PVA), polyacrylic acid and mixtures thereof.

23. The composite thermochemical material according to claim 23, wherein the binder is in the range of up to 5 wt%, such as in the range of 0.25 wt% to 5 wt%, such as 0.5 wt% to 3 wt%.

24. The composite thermochemical material according to any one of claims 16 to 23, further comprising a flow aid, for example a flow aid present in an amount of .

25. A composite thermochemical material according to any one of claims 16 to 24, provided in pellet form, tablet form, extruded form or granular form.

Citation Information

Cited By

  • Thermochemical adsorption heat storage device and heat recovery oxidation system and method

    CN121252544A