A method for preparing a wear-resistant hydrogen storage material with high adsorption capacity
The preparation of metal composites by citric acid sol gel method and combining titanium aluminum carbide and modified diatomaceous earth solves the shortcomings of existing hydrogen storage materials in hydrogen storage capacity, safety and wear resistance, and achieves high efficiency and safety hydrogen storage and transportation.
Patent Information
- Application Number
- CN202411266183.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-11
AI Technical Summary
Existing hydrogen storage materials have shortcomings in hydrogen storage capacity, safety, wear resistance and service life, which is difficult to meet the needs of the hydrogen energy industry, especially in the storage caused by low density, easy leakage, flammable and explosive characteristics of hydrogen. and transportation difficulties.
The metal composites were prepared by citric acid sol gel method, combined with titanium aluminum carbide and modified diatomaceous earth, and by regulating the pH value and proportion, a hydrogen storage material with a high specific surface area and uniform pore size distribution was formed, which improved the catalytic activity of the material and Hydrogen storage properties and enhance the mechanical strength and thermal stability of the material through the calcination and grinding process.
It achieves high hydrogen storage capacity, rapid hydrogen absorption and release kinetic performance, long service life and good mechanical strength, improves the wear resistance and thermal stability of the material, and is suitable for practical applications.
Smart Images

Figure CN118788307B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen energy storage, and relates to a method for preparing a wear-resistant high-adsorption hydrogen storage material. Background Art
[0002] Hydrogen energy is known as the ultimate energy source for mankind in the 21st century. With the continuous growth of global energy demand and the improvement of environmental protection awareness, hydrogen energy, as a clean, efficient and renewable energy source, has received widespread attention. The hydrogen energy industry includes three links: hydrogen production, hydrogen storage and application. Hydrogen is in gaseous state at room temperature and pressure, and has low density, easy leakage, flammable and explosive, which brings great difficulties to storage and transportation. Therefore, the development of efficient and safe hydrogen storage materials is the key to the application of hydrogen energy. Hydrogen storage is the bottleneck currently faced by the industry. Therefore, the invention of a nano hydrogen storage material can effectively enrich the broad orientation of the hydrogen storage industry in material use and selection, and it will prompt researchers in this field to develop new scientific research results.
[0003] There are many hydrogen storage products on the market, generally including methanol hydrogen storage, high-pressure hydrogen storage, liquefied hydrogen storage, solid adsorption hydrogen storage and metal hydride hydrogen storage. Except for high-pressure hydrogen storage, which has been commercialized, other hydrogen storage products are still in the experimental stage. Therefore, how to develop products that can better promote the industry demand for hydrogen storage products and be widely used in the hydrogen storage industry has become an urgent problem for researchers to solve. In view of this, developing a hydrogen storage product with flexible selection, simple structure, high safety, large hydrogen storage capacity, long life, high efficiency and energy saving, and green environmental protection has become a new goal sought by researchers in this field. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a wear-resistant high-adsorption hydrogen storage material, which has the characteristics of strong hydrogen storage capacity and long service life.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a wear-resistant hydrogen storage material with high adsorption capacity, the method for preparing the hydrogen storage material is as follows:
[0007] S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A;
[0008] S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is (1.5-2):1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L;
[0009] S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C;
[0010] S4: introducing ammonia gas with a concentration of 10% into the mixed solution C, and simultaneously raising the temperature to 80°C. When the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D;
[0011] S5: placing gel D in an oven at 110°C for drying for 12 h, transferring the dried solid to a muffle furnace, and calcining at 300°C for 2.5 h to obtain solid E;
[0012] S6: transferring solid E to a ball mill, adding modified diatomaceous earth and titanium aluminum carbide, the mass ratio of which is solid E: modified diatomaceous earth: titanium aluminum carbide = 5:2:2, grinding at a speed of 300 r / min for 1 h to obtain a mixture F;
[0013] S7: The mixture F is transferred to the muffle furnace again, calcined at 400°C for 2 h, cooled to room temperature at a rate of 3°C / min, and then crushed to obtain a powder G with a particle size of 150-200 mesh;
[0014] S8: Powder G is placed in a mold, heated to 1500°C at a rate of 5°C / min, and then reacted at a constant temperature for 8 hours. Then, the powder is cooled to room temperature at a rate of 10°C / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen. The powder is taken out of the mold to obtain the hydrogen storage material.
[0015] Furthermore, the preparation process of the modified diatomite is as follows:
[0016] S1.1: diatomaceous earth and graphene were mixed in a mass ratio of 2:1, and ground in a ball mill at a speed of 400 r / min for 1 h to obtain a mixture H. The mixture H was placed in 10% nitric acid, heated to 60°C, and refluxed for 4 h. After the reaction was completed, it was washed with deionized water to a pH value of 7, and dried at 80°C for 12 h to obtain a mixture I;
[0017] S1.2: Mix the mixture I and zirconium nitrate in a mass ratio of 2:1, heat to 120° C., grind in a ball mill at a speed of 400 r / min for 1 h, introduce nitrogen for purging, and slowly cool to room temperature to obtain the modified diatomite.
[0018] Furthermore, the flow rate of ammonia gas in S4 is 500 ml / min.
[0019] Furthermore, the heating rate of the muffle furnace in S5 is 3°C / min.
[0020] Furthermore, the particle size of the mixture F obtained by grinding in S6 is 200 mesh.
[0021] Furthermore, the heating rate of the muffle furnace in S7 is 5°C / min.
[0022] Furthermore, the particle size of the mixture H obtained by grinding in S1.1 is 200 mesh.
[0023] Furthermore, the nitrogen in said S1.2 has an inlet flow rate of 10 m / s.
[0024] Furthermore, in S1.2, the mixture is slowly cooled to room temperature at a rate of 3°C / min.
[0025] The present invention firstly prepares the metal composite by a citric acid sol-gel method. The sol-gel method has the advantages of controllable structure and uniform composition. The metal composite prepared by the method has the performance of uniform pore size distribution and high specific surface area.
[0026] The complex formed by metal ions such as cerium nitrate, lanthanum nitrate, copper nitrate and citric acid can be evenly dispersed in the sol, ensuring the high dispersion of metal elements in the final hydrogen storage material. The high dispersion of metal elements helps to improve the catalytic activity and hydrogen storage performance of the material. Lanthanum and cerium in the composite metal are both rare earth metals. Rare earth metals have active electronic structures and can react with hydrogen to form stable rare earth hydrides, thereby realizing hydrogen storage. In addition, the uniform dispersion and complexation of metal elements also make the hydrogen storage material have a higher hydrogen storage capacity and faster hydrogen absorption and desorption kinetics.
[0027] During the preparation process, by adjusting the ratio of citric acid to metal ions to (1.5~2):1, ensuring that all metals are complexed, the structure and composition of the material can be better controlled, thereby obtaining a hydrogen storage material with better performance. During the preparation process, ammonia is introduced to control the pH value, which can affect the degree of complexation between citric acid and metal ions and the formation of gel. A pH value of 7 helps to form a stable complex and a uniform gel structure, thereby obtaining a hydrogen storage material with excellent performance; in addition, the material has the best specific surface area and pore size distribution at a pH value of 7, which further improves the hydrogen storage performance of the material.
[0028] Titanium aluminum carbide plays a composite role in hydrogen storage materials, in which titanium and aluminum have strong interactions with hydrogen, while carbon elements provide structural stability. The titanium aluminum carbon compound in titanium aluminum carbide provides a channel for hydrogen diffusion and promotes the diffusion of hydrogen in the hydrogen storage material; titanium carbide is the main carrier for hydrogen storage, and the composite hydrogen storage material obtained by the composite of the two has both good thermodynamic properties of hydrogen storage and release and high hydrogen storage capacity. When titanium aluminum carbide is composited with rare earth metals, the atoms of the two substances diffuse with each other to form a diffusion layer of a certain thickness. The diffusion layer will form a composite interface and allow titanium aluminum carbide to be doped onto the surface of the rare earth metal, which further improves the hydrogen storage performance of the hydrogen storage material. This composite effect can also increase the specific surface area of the material, improve the pore structure, and increase the diffusion rate of hydrogen. The addition of diatomaceous earth can increase the number and pore size of the pores in the hydrogen storage material, which is beneficial to the adsorption and storage of hydrogen. In addition, diatomaceous earth can also be used as a carrier or supporting material to improve the stability and mechanical strength of the hydrogen storage material. The present invention uses modified diatomaceous earth to further enhance its role in hydrogen storage materials.
[0029] First, graphene and diatomaceous earth are mixed in nitric acid at 60°C for reaction. The pH value of the resulting mixture is adjusted to 7, and then mixed with zirconium nitrate, and purged with nitrogen to room temperature to obtain modified diatomaceous earth. In nitric acid, graphene and diatomaceous earth undergo surface modification and chemical bonding to form a tighter bond. This interaction changes the surface properties of diatomaceous earth, increasing its specific surface area and porosity. Graphene's high specific surface area and excellent electron transport properties help increase the adsorption sites of hydrogen molecules, thereby increasing hydrogen storage capacity. Diatomaceous earth itself has a porous structure. After mixing and modifying graphene with it, its structure can be further optimized to provide more hydrogen storage space. Zirconium nitrate is then loaded onto the surface of the diatomite and graphene mixture. The introduction of zirconium nitrate can react with hydroxyl groups, silanol groups, etc. on the surface of diatomite through chemical reactions to form new Si-O-Zr chemical bonds, thereby changing the charge distribution on the surface of the mixture, generating more hydrogen adsorption points, and further optimizing the mixture's pore structure and specific surface area. In addition, this chemical bonding can also enhance the structural stability of the mixture and increase the service life of the hydrogen storage material.
[0030] The addition of modified diatomite and titanium aluminum carbide also improves the thermal stability of the material, which enables the hydrogen storage material to maintain good structure and performance under high temperature conditions, which is conducive to long-term stable operation in practical applications. During the heating process to 1500°C, the organic matter in the material is burned off, and the metal oxides and the added diatomite, titanium aluminum carbide and other components form a stable skeleton structure, giving the hydrogen storage material good mechanical strength.
[0031] Beneficial effects of the present invention:
[0032] The present invention first prepares the metal composite by a citric acid sol-gel method, and by adjusting the ratio of citric acid to metal ions to (1.5-2):1, the prepared metal composite has the properties of uniform pore size distribution and high specific surface area;
[0033] The present invention adds titanium aluminum carbide and rare earth metal composites, and the atoms of the two substances diffuse with each other to form a diffusion layer of a certain thickness. The diffusion layer forms a composite interface and allows titanium aluminum carbide to be doped onto the surface of the rare earth metal, which further improves the hydrogen storage performance of the hydrogen storage material.
[0034] The present invention adds modified diatomaceous earth. First, in nitric acid, graphene and diatomaceous earth undergo surface modification and chemical bonding to form a tighter bond. This interaction changes the surface properties of the diatomaceous earth, increases its specific surface area and porosity, and then is mixed with zirconium nitrate. The synergistic effect between the two further enhances the hydrogen storage performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.
[0036] Figure 1 Example 1 Nitrogen adsorption and desorption curve diagram;
[0037] Figure 2 Comparative Example 1 Nitrogen adsorption and desorption curve;
[0038] Figure 3 Example 1: Pore size distribution diagram. DETAILED DESCRIPTION
[0039] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0040] The preparation process of modified diatomite is as follows:
[0041] S1.1: diatomite and graphene were mixed in a mass ratio of 2:1, and ground in a ball mill at a speed of 400 r / min for 1 h to obtain a mixture H with a particle size of 200 mesh. The mixture H was placed in 10% nitric acid and heated to 60°C, and refluxed for 4 h. After the reaction was completed, it was washed with deionized water to a pH value of 7, and dried at 80°C for 12 h to obtain a mixture I;
[0042] S1.2: Mix the mixture I and zirconium nitrate in a mass ratio of 2:1, heat to 120°C, grind in a ball mill at a speed of 400 r / min for 1 h, introduce nitrogen for purging, and the nitrogen flow rate is 10 m / s. At the same time, slowly cool to room temperature at a rate of 3°C / min to obtain the modified diatomite.
[0043] Example 1
[0044] S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A;
[0045] S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is 1.5:1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L;
[0046] S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C;
[0047] S4: introducing ammonia gas with a concentration of 10% into the mixed solution C at a flow rate of 500 ml / min, and simultaneously raising the temperature to 80° C. After the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D;
[0048] S5: Place gel D in an oven at 110°C for drying for 12 h, transfer the dried solid to a muffle furnace, heat to 300°C at a rate of 3°C / min, and calcine at 300°C for 2.5 h to obtain solid E;
[0049] S6: transferring solid E to a ball mill, adding modified diatomaceous earth and titanium aluminum carbide, the mass ratio of which is solid E: modified diatomaceous earth: titanium aluminum carbide = 5:2:2, grinding at a speed of 300 r / min for 1 h to obtain a mixture F, the particle size of the mixture F is 200 mesh;
[0050] S7: The mixture F is transferred to the muffle furnace again, heated to 400°C at a rate of 5°C / min, calcined at 400°C for 2h, cooled to room temperature at a rate of 3°C / min, and crushed to obtain a powder G with a particle size of 150-200 mesh;
[0051] S8: Powder G is placed in a mold, heated to 1500°C at a rate of 5°C / min, and then reacted at a constant temperature for 8 hours. Then, the powder is cooled to room temperature at a rate of 10°C / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen. The powder is taken out of the mold to obtain the hydrogen storage material.
[0052] Example 2
[0053] S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A;
[0054] S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is 2:1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L;
[0055] S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C;
[0056] S4: introducing ammonia gas with a concentration of 10% into the mixed solution C at a flow rate of 500 ml / min, and simultaneously raising the temperature to 80° C. After the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D;
[0057] S5: Place gel D in an oven at 110°C for drying for 12 h, transfer the dried solid to a muffle furnace, heat to 300°C at a rate of 3°C / min, and calcine at 300°C for 2.5 h to obtain solid E;
[0058] S6: transferring solid E to a ball mill, adding modified diatomaceous earth and titanium aluminum carbide, the mass ratio of which is solid E: modified diatomaceous earth: titanium aluminum carbide = 5:2:2, grinding at a speed of 300 r / min for 1 h to obtain a mixture F, the particle size of the mixture F is 200 mesh;
[0059] S7: The mixture F is transferred to the muffle furnace again, heated to 400°C at a rate of 5°C / min, calcined at 400°C for 2h, cooled to room temperature at a rate of 3°C / min, and crushed to obtain a powder G with a particle size of 150-200 mesh;
[0060] S8: Powder G is placed in a mold, heated to 1500°C at a rate of 5°C / min, and then reacted at a constant temperature for 8 hours. Then, the powder is cooled to room temperature at a rate of 10°C / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen. The powder is taken out of the mold to obtain the hydrogen storage material.
[0061] Comparative Example 1
[0062] S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A;
[0063] S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is 1.5:1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L;
[0064] S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C;
[0065] S4: introducing ammonia gas with a concentration of 10% into the mixed solution C at a flow rate of 500 ml / min, and simultaneously raising the temperature to 80° C. After the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D;
[0066] S5: Place gel D in an oven at 110°C for drying for 12 h, transfer the dried solid to a muffle furnace, heat to 300°C at a rate of 3°C / min, and calcine at 300°C for 2.5 h to obtain solid E;
[0067] S6: transfer the solid E to a ball mill, add diatomaceous earth and titanium aluminum carbide, the mass ratio of which is solid E: diatomaceous earth: titanium aluminum carbide = 5:2:2, grind at a speed of 300 r / min for 1 h to obtain a mixture F, the particle size of the mixture F is 200 mesh;
[0068] S7: The mixture F is transferred to the muffle furnace again, heated to 400°C at a rate of 5°C / min, calcined at 400°C for 2h, cooled to room temperature at a rate of 3°C / min, and crushed to obtain a powder G with a particle size of 150-200 mesh;
[0069] S8: Powder G is placed in a mold, heated to 1500°C at a rate of 5°C / min, and then reacted at a constant temperature for 8 hours. Then, the powder is cooled to room temperature at a rate of 10°C / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen. The powder is taken out of the mold to obtain the hydrogen storage material.
[0070] This comparative example does not use modified diatomaceous earth, but only uses ordinary diatomaceous earth.
[0071] Comparative Example 2
[0072] S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A;
[0073] S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is 1.5:1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L;
[0074] S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C;
[0075] S4: introducing ammonia gas with a concentration of 10% into the mixed solution C at a flow rate of 500 ml / min, and simultaneously raising the temperature to 80° C. After the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D;
[0076] S5: Place gel D in an oven at 110°C for drying for 12 h, transfer the dried solid to a muffle furnace, heat to 300°C at a rate of 3°C / min, and calcine at 300°C for 2.5 h to obtain solid E;
[0077] S6: transferring solid E to a ball mill, adding modified diatomaceous earth, the mass ratio of which is solid E: modified diatomaceous earth = 5:2, grinding at a speed of 300 r / min for 1 h to obtain a mixture F, the particle size of the mixture F is 200 mesh;
[0078] S7: The mixture F is transferred to the muffle furnace again, heated to 400°C at a rate of 5°C / min, calcined at 400°C for 2h, cooled to room temperature at a rate of 3°C / min, and crushed to obtain a powder G with a particle size of 150-200 mesh;
[0079] S8: Powder G is placed in a mold, heated to 1500°C at a rate of 5°C / min, and then reacted at a constant temperature for 8 hours. Then, the powder is cooled to room temperature at a rate of 10°C / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen. The powder is taken out of the mold to obtain the hydrogen storage material.
[0080] In this comparative example, no titanium aluminum carbide was added.
[0081] The wear resistance of Examples 1-2 and Comparative Examples 1-2 was tested by using a JM IV abrasion tester and a rotating friction rubber wheel method. The wear resistance of the present invention was measured by the average value of the coating mass loss (weight loss method) after 100 grinding revolutions. The load was 10 N, the rotation speed was 80 r / min, the test temperature was 25 °C, the relative humidity was 50%, and the mass was tested to an accuracy of 0.01 mg. The average value of 3 measurements was taken as the result. The test results are summarized in the following table.
[0082]
[0083] It can be seen from the experimental data that Example 1 has the best wear resistance, indicating that the addition of modified diatomaceous earth and titanium aluminum carbide improves the wear resistance of the material.
[0084] Nitrogen adsorption and desorption tests were performed on Example 1 and Comparative Example 1 using an instrument model ASAP 2020 HD88 produced by Micromeritics, USA. 2For the adsorption-desorption test, the sample was first pretreated at 200°C under vacuum for 10 h. After the pretreatment, the sample was tested at liquid nitrogen temperature (-196°C). The specific surface area of the catalyst was calculated using the BET model.
[0085]
[0086] The hydrogen storage mass capacity of Example 1 and Comparative Example 1 was tested. The samples were placed in a confined space, a certain flow of hydrogen was introduced and the amount of hydrogen introduced was recorded. After 24 hours, a flow meter was used to record the amount of hydrogen released. The hydrogen storage mass capacity of the material was calculated by the amount of hydrogen introduced and the amount of hydrogen released. The test results are summarized in the following table.
[0087]
[0088] Through the nitrogen adsorption and desorption test of Example 1 and Comparative Example 1, it can be seen that the addition of modified diatomaceous earth makes the material have a larger specific surface area, which makes the material have better hydrogen storage performance. Figure 3 This is the pore size distribution diagram of Example 1. It can be seen from the figure that Example 1 has a prominent peak at 0.55 nm, which indicates that the pore size distribution of Example 1 is uniform.
[0089] The detection of the hydrogen storage mass capacity of the material further verified that Example 1 had better hydrogen storage performance.
[0090] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a wear-resistant high-adsorption hydrogen storage material, characterized in that: The preparation method of the hydrogen storage material is as follows: S1: Cerium nitrate, lanthanum nitrate and copper nitrate were mixed in a molar ratio of 1:1:3, and after mixing evenly, added into deionized water until completely dissolved, and ultrasonicated at room temperature for 0.5 h to obtain a mixed solution A; S2: Weigh citric acid, the molar ratio of citric acid to a mixture of cerium nitrate, lanthanum nitrate and copper nitrate is (1.5-2):1, dissolve the citric acid in deionized water to obtain a solution B with a concentration of 1 mol / L; S3: heating the mixed solution A to 50° C., and slowly adding the solution B to the mixed solution A while stirring until the solution is clear, to obtain a mixed solution C; S4: introducing ammonia gas with a concentration of 10% into the mixed solution C at a flow rate of 500 ml / min, and simultaneously raising the temperature to 80° C. After the pH value of the solution reaches 7, the introduction of ammonia gas is stopped, and stirring is continued to obtain gel D; S5: placing gel D in an oven at 110°C for drying for 12 h, transferring the dried solid to a muffle furnace, and calcining at 300°C for 2.5 h to obtain solid E; S6: transferring solid E to a ball mill, adding modified diatomaceous earth and titanium aluminum carbide, the mass ratio of which is solid E: modified diatomaceous earth: titanium aluminum carbide = 5:2:2, grinding at a speed of 300 r / min for 1 h to obtain a mixture F; S7: The mixture F is transferred to the muffle furnace again, calcined at 400°C for 2 h, cooled to room temperature at a rate of 3°C / min, and then crushed to obtain a powder G with a particle size of 150-200 mesh; S8: Powder G is placed in a mold, heated to 1500° C. at a rate of 5° C. / min, and then subjected to constant temperature reaction for 8 hours after the temperature reaches 1500° C., and then cooled to room temperature at a rate of 10° C. / min in a nitrogen atmosphere, and allowed to stand at room temperature for 2 hours while continuously purging with nitrogen, and then taken out from the mold to obtain the hydrogen storage material; The preparation process of the modified diatomite is as follows: S1.1: diatomaceous earth and graphene were mixed in a mass ratio of 2:1, and ground in a ball mill at a speed of 400 r / min for 1 h to obtain a mixture H. The mixture H was placed in 10% nitric acid, heated to 60°C, and refluxed for 4 h. After the reaction was completed, it was washed with deionized water to a pH value of 7, and dried at 80°C for 12 h to obtain a mixture I; S1.2: Mix the mixture I and zirconium nitrate in a mass ratio of 2:1, heat to 120° C., grind in a ball mill at a speed of 400 r / min for 1 h, introduce nitrogen for purging, and slowly cool to room temperature to obtain the modified diatomite.
2. The method for preparing a wear-resistant and high-adsorption hydrogen storage material according to claim 1, characterized in that: The heating rate of the muffle furnace in S5 is 3°C / min.
3. The method for preparing a wear-resistant and high-adsorption hydrogen storage material according to claim 1, characterized in that: The particle size of the mixture F obtained by grinding in S6 is 200 mesh.
4. The method for preparing a wear-resistant and high-adsorption hydrogen storage material according to claim 1, characterized in that: The heating rate of the muffle furnace in S7 is 5°C / min.
5. The method for preparing a wear-resistant and high-adsorption hydrogen storage material according to claim 1, characterized in that: The particle size of the mixture H obtained by grinding in S1.1 is 200 mesh.
6. The method for preparing a wear-resistant and high-adsorption hydrogen storage material according to claim 1, characterized in that: The nitrogen inlet flow rate in S1.2 is 10 m / s.
7. The method for preparing a wear-resistant high-adsorption hydrogen storage material according to claim 1, characterized in that: In the S1.2, the mixture was slowly cooled to room temperature at a rate of 3°C / min.