Sintered carbonized material as well as preparation method and application thereof
By filling the pores of the sintered matrix with polymer compounds and performing high-temperature carbonization treatment, the problems of density reduction and cementite formation during friction reduction of existing iron-based/copper-based sintered materials are solved, achieving better friction reduction and Performance improvements.
Patent Information
- Application Number
- CN202410785801.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
AI Technical Summary
When existing iron-based/copper-based sintered materials are used to reduce friction, the addition of graphite leads to a reduction in density and the formation of cementite, which affects the overall performance of the material. Moreover, it is difficult to effectively reduce the friction coefficient with existing methods to improve the life and energy consumption efficiency of mechanical parts. .
By filling the pores of the sintered matrix with a polymer compound or mixture as an impregnation agent, the pyrolysis is performed to form carbonized substances, and solid or liquid impregnation agents are used to infiltrate and carbonize in a protective atmosphere to ensure deep filling and temperature control of the carbonized substances. Avoid cementite formation.
It improves the friction reducing effect of iron-based sintered materials, maintains material density, reduces friction coefficient, extends the life of mechanical parts and improves energy consumption efficiency.
Smart Images

Figure CN118788964A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of powder metallurgy sintered materials, and in particular relates to an iron-based / copper-based sintered carbonized material and a preparation method and application thereof. Background Art
[0002] Powder metallurgy sintered materials are suitable for producing products of the same shape and quantity. They require little or no subsequent mechanical processing, so they can greatly save metal and reduce product costs. In addition, because their mechanical properties are comparable to those of casting materials and can be adjusted within a larger range according to requirements, their use is increasing in many fields such as transportation machinery, agricultural machinery, and textile machinery, making them an indispensable basic component material in the machinery industry.
[0003] Among the powder metallurgy sintered materials, iron-based and copper-based materials are the most widely used. Since powder metallurgy sintered materials have pores inside, they have good tribological properties after being impregnated with oil. Therefore, iron-based / copper-based sintered materials are usually used as anti-friction materials. With the development of modern industry and the deepening of the concept of green development, the requirements for anti-friction materials have also been further improved, and it is necessary to further reduce the friction coefficient and increase the life of parts and the energy consumption of machinery.
[0004] Since there are pores in powder metallurgy sintered materials, the friction reduction effect is usually achieved by oiling, sulfurizing or adding graphite in the pores. The method of adding graphite to sintered materials is generally to directly add graphite when the sintered materials are mixed with powder, but it will affect the density of the pressed green sheet when the sintered materials are pressed, resulting in a lower density of the pressed green sheet, and the density of the pressed green sheet after sintering will also be low, which will reduce the comprehensive performance of the material. In addition, after adding graphite when the iron-based sintered materials are mixed with powder, during sintering, due to the high carbon content, more cementite is easily generated, and the cementite is mostly distributed at the grain boundaries, which will cause the plastic toughness of the material to decrease, and the tensile strength to decrease, which is not conducive to the comprehensive performance of the material. Summary of the invention
[0005] The purpose of the present invention is to provide an iron-based / copper-based sintered carbonized material and a preparation method thereof, so as to improve the friction reduction effect of the iron-based sintered material.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] The first inventive object of the present invention is to provide a sintered carbonized material, the matrix of which is an iron-based material or a copper-based material, the microstructure of which has pores, the pores are filled with a carbonized substance, and the carbonized substance is a solid product after the infiltrant penetrates into the matrix and is decomposed at high temperature.
[0008] In a further embodiment, the impregnating agent is a polymer compound or a mixture, and the carbonized material is filled into the pores to a depth of ≥0.2 mm.
[0009] The second object of the present invention is to provide a method for preparing the above-mentioned sintered carbonized material, comprising the following steps:
[0010] (1) preparing a sintered substrate;
[0011] The method comprises mixing, pressing and sintering raw materials to prepare a sintered matrix;
[0012] (2) Infiltration treatment with an infiltrant: infiltrating the infiltrant into the pores of the sintered matrix, wherein the infiltrant is a polymer compound or a mixture; during the infiltration treatment, the depth of the infiltrant in the sintered matrix is ≥ 0.2 mm;
[0013] The impregnant includes a solid impregnant and a liquid impregnant;
[0014] When a solid infiltrant is used, the solid infiltrant is coated on the surface of the sintered substrate; under a protective atmosphere, it is heated to the melting temperature of the solid infiltrant to melt the solid infiltrant and infiltrate into the pores of the sintered substrate.
[0015] In a further embodiment, the coating is to electrostatically spray, liquid-brush or powder-sheet coating the solid impregnant, wherein the liquid-brush coating is to dissolve the solid impregnant into a liquid or suspension and then brush it onto the surface of the sintered substrate. Electrostatic spraying, liquid-brush or powder-sheet coating are all conventional coating methods in the art.
[0016] When using a liquid impregnant, place the sintered substrate in an impregnation box, evacuate the box, and then inject the liquid impregnant to allow the impregnant to enter the pores of the sintered substrate; or soak the sintered substrate in the liquid impregnant for 3-30 minutes to allow the impregnant to enter the pores of the sintered substrate.
[0017] (3) Carbonization:
[0018] The sample after the above treatment is heated to the carbonization temperature under a protective atmosphere to carbonize the infiltrant in the pores of the sintered matrix to obtain a sintered carbonized material.
[0019] When a solid infiltrant is used, continue heating after heating to the melting temperature of the solid infiltrant in the previous step, or keep warm for a period of time or cool and then continue heating, the heating temperature is raised to the carbonization temperature of the solid infiltrant to carbonize the infiltrant, and the heating rate is ≤12°C / min;
[0020] When a liquid impregnant is used, the liquid impregnant is heated to the curing temperature of the liquid impregnant to cure the liquid impregnant in the pores of the sintered matrix. In this application, heating to the curing temperature of the liquid impregnant means heating to the curing temperature in a water bath, air or protective atmosphere, and the curing temperature is 70°C-150°C. Then continue to heat or keep warm for a period of time or continue to heat after cooling to raise the temperature to the carbonization temperature to carbonize the impregnant.
[0021] Since the liquid infiltrant has penetrated into the pores of the sintered matrix, the heating process during the carbonization process is a slow heating process with a heating rate of ≤12°C / min. When passing through the solidification temperature range, the infiltrant will solidify and does not require specific insulation settings or water bath heating.
[0022] The carbonization process of the impregnating agent is a process in which a polymer compound or a mixture is decomposed by heat. The polymer compound or the mixture is decomposed by heat, losing all or part of substances such as O and H, leaving part of the solid C or a combination of C.
[0023] The solid impregnation agent described in the present application can be selected from a polyphenylene sulfide mixture, wherein the weight fraction of polyphenylene sulfide is ≥70%, and the other components are thermoplastic polymer compounds with a melting point less than 400°C, such as nylon, polyetheretherketone, etc.; the combination includes weight fractions of polyphenylene sulfide 70% + polyetheretherketone 30%, polyphenylene sulfide 80% + PA6 (polyamide 6) 20%, etc.
[0024] The liquid infiltrant contains a curing agent and is a commercially available infiltrant for powder metallurgy products or castings, such as Permaseal C-2005 infiltrant, GODER-1890 infiltrant, and the like.
[0025] The third invention objective of the present invention is to provide the use of the sintered carbonized material for preparing mechanical parts, including but not limited to: sliding bearings, vane pump or plunger pump oil distribution plates, gear pump side plates, and car air conditioner swash plates. After the carbonization process, the mechanical parts may also include an oil immersion process, a shaping process, and a machining process.
[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0027] Since the sintered matrix contains pores, the present application uses an infiltration method to allow the infiltrant to infiltrate the pores of the sintered matrix, and the infiltration treatment process is after the pressing process of the sintered matrix, so it will not affect the density during pressing.
[0028] In addition, the impregnation agent in the present application is selected as a polymer compound or a mixture, which will decompose when heated during the carbonization process. The polymer compound or the mixture decomposes when heated, loses all or part of O and H, and leaves a part of solid C or C combination.
[0029] In the present application, the carbonization temperature is 300°C-700°C. Specifically, the carbonization temperature of the liquid impregnant is 300°C-600°C; the carbonization temperature of the solid impregnant is 400°C-700°C. If the carbonization temperature is too high, the carbon will form more free activated carbon at high temperature, and the amount of carbon left in the pores will be very small, thus affecting the friction reduction effect; if it is an iron-based material, the temperature is too high, and cementite is easy to form; if it is a copper-based material, deformation may occur if the temperature is too high; if the carbonization temperature is low, the infiltrant in the pores of the sintered matrix is not easy to carbonize. Therefore, the carbonization temperature in the present application is not easy to form cementite while ensuring that the infiltrant is carbonized. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the organization diagram of the carbonized material prepared in Example 2;
[0031] Figure 2 This is the distribution of carbon components in the material structure of Example 2. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below with reference to the embodiments.
[0033] Embodiment 1:
[0034] A method for preparing a sintered carbonized material comprises the following steps:
[0035] (1) Preparation of sintered matrix:
[0036] Weighing materials: weigh 90 parts of reduced iron powder, 10 parts of copper powder, 0.5 parts of graphite, 0.8 parts of zinc stearate, and 0.05 parts of spindle oil according to the weight ratio;
[0037] Mixing: Use a double cone mixer to mix evenly;
[0038] Pressing: Pressing density is 6.2-6.3g / cm 3 The diameter of the disc specimen is 36mm;
[0039] Sintering: sintering at 1120°C for 40 minutes to prepare a sintered matrix;
[0040] (2) Impregnation treatment with impregnant: The liquid impregnant is GODER-1890 type impregnant
[0041] Place the sintered substrate in an impregnation box, evacuate the chamber to a vacuum value of <-25in Hg, and then inject the liquid impregnant to allow the impregnant to enter the pores of the sintered material;
[0042] (3) Carbonization: The impregnated material is heated in a water bath to solidify the liquid impregnant in the pores of the sintered matrix. The solidification temperature is 85°C and the time is 30 minutes.
[0043] The solidified material was placed in a tubular furnace and heated to 600°C at a heating rate of 12°C / min in a nitrogen and hydrogen atmosphere and kept at this temperature for 30 minutes to carbonize the infiltrant in the pores of the sintered matrix to obtain a sintered carbonized material.
[0044] Embodiment 2:
[0045] (1) Preparation of sintered substrate: Same as Example 1 (density of sintered substrate is 6.2-6.6 g / cm 3 ),
[0046] (2) Infiltration treatment with infiltration agent: The liquid infiltration agent is Permaseal C-2005 type infiltration agent. The sintered substrate is immersed in the liquid infiltration agent for 10 minutes to allow the infiltration agent to enter the pores of the sintered material.
[0047] (3) Carbonization: The impregnated material is placed in a tubular furnace and slowly heated in a nitrogen and hydrogen atmosphere to 70°C-150°C to solidify the liquid impregnant in the pores of the sintered matrix. The temperature is then raised to 300°C at a rate of 12°C / min and kept at this temperature for 30 minutes to carbonize the impregnant in the pores of the sintered matrix to obtain a sintered carbonized material.
[0048] The sintered carbonized material prepared in this embodiment was observed for its structure. The composition analysis was performed using a Zeiss sigma300 field emission scanning electron microscope and an energy dispersive spectrometer. Before the observation, the material was degreased according to GB / T 8643 "Soxhlet extraction method for determination of lubricant content in lubricant-containing metal powders" to extract the lubricating oil in the pores of the material. The electron microscope scanning image is shown in FIG. Figure 1 As shown, the carbon component (red part) analyzed by the energy spectrometer is distributed as follows Figure 2 As shown by Figure 1 and Figure 2 By comparison, it can be seen that the carbon component (red part) is distributed in the pores of the sintered matrix.
[0049] Embodiment 3:
[0050] (1) Preparation of sintered matrix:
[0051] Weighing materials: weigh 100 parts of 1300WB diffusion alloy steel powder (Mo: 0.5-0.7wt%, Ni: 1.7-2.1wt%, Cu: 1.4-1.6wt%, Fe balance), 0.7 parts of graphite, 0.8 parts of zinc stearate, and 0.05 parts of spindle oil according to the weight ratio;
[0052] Mixing: Use a double cone mixer to mix evenly;
[0053] Pressing: Pressing density is 6.6-6.7g / cm 3The diameter of the disc specimen is 36mm;
[0054] Sintering: Sintering at 1120°C for 40 min to prepare a sintered matrix (the density of the sintered matrix is 6.6-6.7 g / cm 3 );
[0055] (2) Impregnation treatment with impregnation agent: The solid impregnation agent is in powder form and its composition is 70% polyphenylene sulfide + 30% polyetheretherketone;
[0056] A solid impregnant layer with a thickness of 0.06 mm is coated on the sintered substrate by electrostatic spraying; the sample is placed in a vacuum atmosphere and kept at 315°C for 30 minutes to melt the solid impregnant and enter the pores of the sintered substrate;
[0057] (3) Carbonization: After the infiltration is completed, continue heating to raise the temperature to 400°C and keep it warm for 30 minutes to carbonize the infiltrant in the pores of the sintered matrix. Then cool it with the furnace to obtain a sintered carbonized material.
[0058] The carbonized materials prepared in Examples 1-3 were made into test specimens, and the test was repeated four times. The specimens of Example 1 are S1-1 to S1-4, the specimens of Example 2 are S2-1 to S2-4, and the specimens of Example 3 are S3-1 to S3-4. The specimens prepared in each step were weighed. The sintered substrate was weighed before the infiltration treatment with the infiltrant, and its weight was calculated as the sintering weight; after the infiltration treatment with the infiltrant, the product was weighed, and the difference with the sintering weight was calculated as the infiltration amount; the carbonized product was weighed, and the difference with the sintering weight was calculated as the carbonization amount. The details are shown in Table 1:
[0059] Table 1
[0060] Repeat the experiment Sintered weight (g) Impregnation amount (g) Carbonization amount (g) S1-1 24.32 0.98 0.07 S1-2 24.26 0.98 0.08 S1-3 24.36 0.99 0.07 S1-4 24.38 0.97 0.06 S2-1 24.33 0.86 0.51 S2-2 24.35 0.85 0.47 S2-3 24.36 0.80 0.48 S2-4 24.27 0.82 0.49 S3-1 25.10 0.18 0.12 S3-2 25.14 0.17 0.11 S3-3 25.09 0.19 0.12 S3-4 25.13 0.16 0.11
[0061] It can be seen from Table 1 that the average carbonization amount in Example 1 of the present application is 0.07g, and the average carbonization amount in Example 2 is 0.49g. The carbonization temperature of Example 1 is 600°C, which is significantly higher than 300°C in Example 2, indicating that the carbonization temperature affects the carbonization amount. High temperature will cause the carbon after carbonization of the impregnant in Example 1 to form more free activated carbon at high temperature, and the amount of carbon left in the pores of the sintered matrix will become less.
[0062] The average carbonization amount in Example 3 is 0.115 g. Compared with Example 2, the carbonization temperature is similar, but the sintered substrates in these two examples are different. The density of the sintered substrate in Example 3 is 6.6-6.7 g / cm 3 , while the density of the sintered matrix in Example 2 is 6.2-6.6 g / cm 3That is, the density of the sintered matrix in Example 3 is large, and its porosity is relatively small, so the amount of the infiltrant infiltrating into the sintered matrix is small; in addition, a solid infiltrant is selected in Example 3, and its penetration depth into the pores of the sintered matrix is shallower. Therefore, after heating and carbonization, the carbonization amount in Example 3 is lower than that in Example 1.
[0063] In Examples 1-3, the depth of the carbonized material filling the pores was ≥ 0.2 mm as observed by scanning electron microscopy.
[0064] Comparative Example 1:
[0065] (1) Preparation of sintered matrix:
[0066] Weighing materials: weigh 90 parts of reduced iron powder, 10 parts of copper powder, 0.5 parts of graphite, 0.8 parts of zinc stearate, and 0.05 parts of spindle oil according to the weight ratio;
[0067] Mixing: Use a double cone mixer to mix evenly;
[0068] Pressing: Pressing density is 6.2-6.3g / cm 3 The diameter of the disc specimen is 36mm;
[0069] Sintering: sintering at 1120°C for 40 minutes to prepare a sintered matrix;
[0070] (2) Heating: Place the sintered substrate in a tubular furnace and heat to 600°C at a heating rate of 12°C / min in a nitrogen and hydrogen atmosphere and keep the temperature for 30 min.
[0071] Comparative Example 2:
[0072] (1) Preparation of sintered substrate: Same as in Example 1,
[0073] (2) Oil impregnation treatment: Place the sintered substrate in an impregnation box, evacuate the chamber to a vacuum level of <-25 in Hg, and then inject L-AN 32 lubricating oil to allow the lubricating oil to enter the pores of the sintered material;
[0074] (3) Carbonization: The oil-impregnated material is placed in a tubular furnace and heated to 600°C at a heating rate of 12°C / min in a nitrogen and hydrogen atmosphere and kept at this temperature for 30 minutes.
[0075] Comparative Example 3:
[0076] (1) Preparation of sintered matrix: Weighing materials: Weigh 100 parts of 1300WB diffusion alloy steel powder, 0.7 parts of graphite, 0.8 parts of zinc stearate, and 0.05 parts of spindle oil according to weight ratio;
[0077] Mixing: Use a double cone mixer to mix evenly;
[0078] Pressing: Pressing density is 6.6-6.7g / cm 3 The diameter of the disc specimen is 36mm;
[0079] Sintering: sintering at 1120°C for 40 minutes to prepare a sintered matrix;
[0080] (2) Heating: Place the sample in a vacuum atmosphere, keep it at 315°C for 30 min, then increase the temperature to 400°C at a rate of 12°C / min, keep it at that temperature for 30 min, and then cool it in the furnace.
[0081] The carbonized materials prepared in the above-mentioned Examples 1-3 and Comparative Examples 1 and 3 were used to make test specimens.
[0082] The tribological properties of the materials prepared in Example 1 and Comparative Example 1 in this application were tested as follows:
[0083] HDM-200 friction and wear tester was used. The wear part was rotated, the sample was placed stationary, and positive upward pressure was applied to the lower end of the sample to form sliding friction between the sample and the wear part. L-AN 32 lubricating oil was selected and placed on the test base. The friction surface of the wear part was a torus with an inner diameter of 22mm and an outer diameter of 30mm. Four 2mm wide oil grooves were evenly distributed on the torus. The surface of the sample was flat-ground Ra0.4-Ra0.8. The friction and wear performance of the sample was tested. The initial load was 800N, the loading amplitude was 200N / 10min, and the test was stopped when the oil temperature exceeded 120℃ or the friction torque exceeded 5NM. Since the friction and wear test is generally highly dispersed, 4 repeated tests were performed, and the test results were averaged, retaining three significant figures.
[0084] The friction and wear test results of Example 1 and Comparative Example 1 are shown in Table 2, wherein S1-1 to S1-4 are the test results of Example 1, and D1-1 to D1-4 are the test results of Comparative Example 1.
[0085] Table 2 Friction and wear test results of Example 1 / Comparative Example 1
[0086] S1-1 S1-2 S1-3 S1-4 D1-1 D1-2 D1-3 D1-4 Friction factor 0.093 0.095 0.090 0.095 0.096 0.093 0.096 0.101 Test duration min 81 78 92 82 76 80 63 74 Final temperature℃ 121 119 121 116 121 121 110 121
[0087] Comparing Example 1 with Comparative Example 1, it is found that in Example 1, the average friction coefficient of 4 tests is 0.09325, the maximum friction coefficient is 0.095, the minimum friction coefficient is 0.090, the average test time is 83.25min, the maximum test time is 92min, and the minimum test time is 78min. In Comparative Example 1, the average friction coefficient of 4 tests is 0.0965, the maximum friction coefficient is 0.101, the minimum friction coefficient is 0.093, the average test time is 73.25min, the maximum test time is 80min, and the minimum test time is 63min. Therefore, Example 1 of the present application is improved relative to Comparative Example 1 in terms of average friction coefficient, maximum friction coefficient, minimum friction coefficient, average test time, maximum test time and minimum test time, and the improvement effect is not significant because the amount of carbonization is small.
[0088] In addition, the average friction coefficient of the sintered carbonized material of Example 1 is reduced by 0.00325 compared with that of Comparative Example 1, that is, the friction coefficient of the sintered carbonized material of Example 1 is reduced by 0.00325 / 0.0965*100%=3.37%.
[0089] In Comparative Example 2, the impregnation agent selected L-AN 32 lubricating oil to impregnate the sintered substrate, and the amount of impregnation oil was about 0.6 g. After heating at 600°C, the weight of the final product was basically consistent with the sintered weight, and the increase was very small and negligible, as shown in Table 3. This indicates that the L-AN 32 lubricating oil did not carbonize the residual carbonized material in the pores of the sintered substrate.
[0090] GB / T 5163-2006 "Determination of density, oil content and porosity of sintered metal materials (excluding cemented carbide)" also points out: In practical applications, there are many methods for degreasing (such as heating under a protective atmosphere). When there is a dispute, the Soxhlet extraction method is used as the standard method. It can be seen that after degreasing by heating, it is very difficult to leave carbonized substances in the pores of the sintered material.
[0091] Table 3
[0092] Repeat the experiment Sintered weight (g) Immersion oil volume (g) Increase after carbonization (g) D2-1 24.34 0.6 -0.01 D2-2 24.30 0.62 0.01 D2-3 24.31 0.61 0.01 D2-4 24.26 0.63 0
[0093] The friction factor test method in Example 3 and Comparative Example 3 of the present application is: using a ring-block friction wear test, the standard is GB / T 12444-2006 "Metallic Material Wear Test Method Test Ring-Test Block Sliding Wear Test", the loading force is 20Kg, the rotation speed is 400r / min, oil dripping lubrication, and the oil dripping amount is 3-5 drops per minute. Since the friction and wear test is generally highly dispersed, 4 repeated tests are performed, and the average value is calculated for each test, retaining three significant digits. Each test lasts 65 minutes, and the values are recorded from 5 minutes, and recorded once at 5 / 10 / 15 / 20 / 30 / 40 / 50 / 60 minutes of the test. The friction and wear test results of Example 3 and Comparative Example 3 are shown in Table 4, where S3-1 to S3-4 are the test results of Example 3, and D3-1 to D3-4 are the test results of Comparative Example 3.
[0094] Table 4 Friction and wear test results of Example 3 and Comparative Example 3
[0095] Serial number 5min 10min 15min 20min 30min 40min 50min 60min average S3-1 0.078 0.076 0.075 0.075 0.073 0.070 0.068 0.065 0.073 S3-2 0.079 0.071 0.071 0.068 0.069 0.065 0.065 0.065 0.069 S3-3 0.075 0.073 0.070 0.068 0.065 0.063 0.063 0.060 0.067 S3-4 0.078 0.074 0.070 0.070 0.065 0.063 0.063 0.060 0.068 D3-1 0.093 0.091 0.091 0.088 0.085 0.078 0.075 0.073 0.084 D3-2 0.090 0.093 0.091 0.090 0.085 0.080 0.073 0.073 0.084 D3-3 0.096 0.095 0.095 0.093 0.090 0.085 0.081 0.081 0.090 D3-4 0.088 0.088 0.086 0.08 0.078 0.074 0.074 0.074 0.080
[0096] It can be clearly seen from Table 4 that the friction coefficient of the material prepared in Example 3 is significantly smaller than the friction coefficient of the material prepared in Comparative Example 3, indicating that the friction reduction performance of the sintered carbonized material prepared in the present invention is improved.
[0097] The average friction coefficients of Example 3 and Comparative Example 3 are 0.069 and 0.085 respectively. The friction coefficient of the material of Example 3 is reduced by 0.016, that is, it is reduced by 0.016 / 0.085*100%=18.82%, which is a significant reduction.
[0098] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to the implementation cases and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the implementation cases herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A sintered carbonized material, the matrix of which is an iron-based material or a copper-based material, and the microstructure of the matrix has pores, Features: The pores are filled with carbonized material, which is a solid product after the infiltrant penetrates into the matrix and is decomposed at high temperature.
2. A sintered carbonized material according to claim 1, Features: The impregnating agent is a polymer compound or a mixture, and the depth of the carbonized material filled in the pores is ≥0.2 mm.
3. A method for preparing a sintered carbonized material, Features: The following steps are involved: (1) preparing a sintered substrate; (2) Infiltration treatment with an infiltrant: infiltrating an infiltrant into the pores of the sintered matrix, wherein the infiltrant is a polymer compound or a mixture; (3) Carbonization: Heating to the carbonization temperature under a protective atmosphere to carbonize the infiltrant in the pores of the sintered matrix to obtain a sintered carbonized material.
4. The preparation method according to claim 3, Features: The sintered matrix is prepared by mixing, pressing and sintering raw materials; the sintered matrix is an iron-based or copper-based sintered matrix.
5. The preparation method according to claim 3, Features: The penetration depth of the infiltrant into the sintered matrix is ≥0.2 mm; and the carbonization temperature is 300° C.-700° C.
6. The preparation method according to claim 3, Features: The impregnating agent includes a solid impregnating agent and a liquid impregnating agent. The solid impregnating agent is a polyphenylene sulfide powder mixture, wherein the weight fraction of polyphenylene sulfide is ≥70%; and the liquid impregnating agent is an impregnating agent for powder metallurgy products or castings.
7. The preparation method according to claim 6, Features: When the infiltrant is a solid infiltrant, the solid infiltrant is coated on the surface of the sintered substrate and heated to the melting temperature of the solid infiltrant under a protective atmosphere to melt the solid infiltrant and infiltrate into the pores of the sintered substrate.
8. The preparation method according to claim 6, Features: When the impregnant is a liquid impregnant, the sintered substrate is placed in an impregnation box, vacuumed, and then the liquid impregnant is injected to allow the impregnant to enter the pores of the sintered substrate; Alternatively, the sintered substrate is immersed in a liquid infiltrant for 3-30 minutes to allow the infiltrant to enter the pores of the sintered material.
9. The preparation method according to claim 8, Features: The coating is electrostatic spraying, liquid painting or powder sheet covering.
10. Use of the sintered carbonized material according to claim 1 or 2, Features: The invention is used for preparing mechanical parts, and the mechanical parts include sliding bearings, vane pump oil distribution plates, plunger pump oil distribution plates, gear pump side plates or automobile air conditioner inclined plates.