Precise iron-chromium-aluminum alloy strip welding method
By using beryllium copper alloy electrodes and water-cooling lubrication technology, combined with appropriate welding process parameters, the problem of weld cracking caused by poor welding of precision iron-chromium-aluminum alloy strips has been solved, and the stability of high-temperature welding and welding quality have been improved.
Patent Information
- Application Number
- CN202411146576.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-18
AI Technical Summary
Poor welding of precision iron-chromium-aluminum alloy strips during the bright annealing process causes weld cracking, which increases the risk of strip breakage. The oxide film hinders metal bonding at high temperatures and complicates the welding process.
It uses beryllium copper alloy electrodes with built-in water-cooling lubrication. Through appropriate welding current, speed, pressure and weld size technology, the welding process is controlled, thermal stress and heat loss are reduced, and the welding is ensured to be firm.
It effectively solves the problem of weld cracking in the furnace, ensures welding quality, avoids strip breakage in the furnace, and improves the reliability and consistency of welding.
Smart Images

Figure CN118789088A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of precision alloy strip production, and in particular to a precision iron-chromium-aluminum alloy strip welding method. Background Art
[0002] When bright annealing precision iron-chromium-aluminum alloy strips, the tail of the previous strip needs to be welded to the head of the next strip to achieve continuous operation of the strip. The conventional welding method for precision alloy strips is to overlap the head and tail for resistance welding, clamp the overlapping part between the upper and lower electrodes, pass a large current, so that the contact part quickly heats up and melts to form a molten core, thereby welding the strips together.
[0003] Iron-chromium-aluminum alloy is different from other alloy strips. Its resistivity is higher, which is more than ten times that of ordinary stainless steel strips. This requires that the current density of resistance welding should be much higher than that of ordinary stainless steel strips. At the same time, the iron-chromium-aluminum alloy strips have the following characteristics that make them unfavorable for welding: 1. The thermal expansion coefficient of iron-chromium-aluminum alloy is relatively high, and large thermal stress will be generated during welding, thereby increasing the risk of weld cracking. 2. Iron-chromium-aluminum alloy materials have good thermal conductivity, which makes the heat dissipation rate in the welding area faster. If the welding process is not properly controlled, it may cause the weld to cool too quickly, affecting the quality of the welded joint. 3. At high temperatures, a dense oxide film is easily formed on the surface of iron-chromium-aluminum alloy, which hinders the good bonding between metals and increases the complexity of the welding process.
[0004] Based on the above problems, it is necessary to develop a resistance welding method for iron-chromium-aluminum alloy strips to ensure that the welding is firm and not easy to open under high temperature conditions in the annealing furnace, thereby avoiding the strip from breaking in the furnace.
[0005] The present invention aims to solve the key problem encountered when annealing precision iron-chromium-aluminum alloy strips in a vertical bright annealing furnace - weld cracking due to poor welding and strip breakage in the furnace. In order to overcome the deficiencies in the prior art, the present invention provides a resistance welding method suitable for iron-chromium-aluminum alloy strips, which achieves effective welding of precision iron-chromium-aluminum alloy strips by adopting suitable welding current, speed, pressure, weld size and other welding processes, selecting beryllium copper alloy electrodes suitable for high-temperature welding, and having built-in water cooling and lubrication in the electrodes, thereby solving the problem of weld cracking in the furnace. Summary of the invention
[0006] The purpose of the present invention is to provide a precision iron-chromium-aluminum alloy strip welding method in view of the above problems.
[0007] The object of the present invention is achieved as follows: 1. A precision iron-chromium-aluminum alloy strip welding method, comprising the following aspects: (1) welding process: the electrode is a plate electrode, the strip is overlapped and laid on the electrode, the upper electrode is a wheel electrode, rolling on the surface of the strip, and the welding wheel rolls from one side of the strip to the other side during welding. During welding, three-phase AC enters the medium frequency inverter, and after rectification-filtering-inversion, the medium frequency AC voltage is output to the medium frequency transformer, and then the medium frequency transformer is stepped down-rectified and the medium frequency DC is output to the welding machine electrode; (2) electrode selection: the electrode material is beryllium copper, and the properties of the selected beryllium copper material after heat treatment are as follows: hardness HV: 400~450, conductivity IACS: 80%~85%, softening temperature ℃: 930~950.
[0008] The welding process parameters are: strip thickness mm: 0.02 ~ 0.03, current kA: 2 ~ 4.5, speed m / min: 8 ~10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.03 ~ 0.05, current kA: 3.6 ~ 6, speed m / min: 8 ~10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.05 ~ 0.1, current kA: 4.5 ~ 9, speed m / min: 8 ~10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.1 ~ 0.25, current kA: 7.2 ~ 18, speed m / min: 6 ~8, pressure bar: 5, weld width mm: 5; strip thickness mm: 0.25 ~ 0.5, current kA: 15 ~ 30, speed m / min: 6 ~8, pressure bar: 5, weld width mm: 5; strip thickness refers to the thickness of the single piece of the overlapping part of the head and tail of the strip, and the welding machine speed refers to the speed of the welding wheel. The welding pressure refers to the pressure of the welding wheel on the surface of the strip through the cylinder lifting and lowering. The weld width is determined by the width of the upper electrode welding wheel. The thickness difference between the two strips welded together should not exceed 30% of the total thickness.
[0009] A circulating cooling water channel is arranged inside the welding wheel and the plate electrode to reduce the high temperature generated by welding.
[0010] Clean the strip surface before welding. The standard is: the residual oil on one side is less than 300mg / m 2 , the iron powder residue on one side is less than 100 mg / m 2 .
[0011] The beneficial effects of the present invention are as follows: the present invention provides a resistance welding method suitable for iron-chromium-aluminum alloy strips, which realizes effective welding of precision iron-chromium-aluminum alloy strips by adopting welding processes such as appropriate welding current, speed, pressure, weld size, etc., selecting beryllium-copper alloy electrodes suitable for high-temperature welding, and having built-in water cooling and lubrication of the electrodes, thereby solving the problem of strip breakage caused by cracking of the weld in the furnace. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The present invention will be further described below in conjunction with the accompanying drawings.
[0013] Figure 1 It is a schematic diagram of precision iron-chromium-aluminum strip resistance welding.
[0014] 1-pressing cylinder, 2-circulating cooling water, 3-upper electrode, 4-strip one, 5-lower electrode, 6-strip two. DETAILED DESCRIPTION
[0015] The present invention provides a method for welding a precision iron-chromium-aluminum alloy strip, which includes the following parts: 1. Welding process: The lower electrode of the present invention is a plate electrode, and the strip is laid on the electrode after overlapping, and the upper electrode is a wheel electrode, which rolls on the surface of the strip. During welding, the welding wheel rolls from one side of the strip to the other side. During welding, three-phase AC enters the medium frequency inverter, and after rectification-filtering-inversion, the medium frequency AC voltage is output to the medium frequency transformer, and then the medium frequency DC is output to the welding machine electrode after voltage reduction-rectification by the medium frequency transformer. The welding process is shown in Table 1.
[0016]
[0017] In Table 1, "applicable strip thickness" refers to the thickness of the single piece at the overlapping part of the head and tail of the strip. When the thickness of the two single pieces is the same, the process in the table should be used.
[0018] In Table 1, the current is a range value, and the material within the thickness range can use any current value within this range according to the actual situation.
[0019] The thickness difference between the two strips welded together should not exceed 30% of the total thickness, otherwise there is a risk of breakdown or poor welding.
[0020] If the thickness of the two strips is inconsistent, the thicker strip should be used as the basis for selecting the parameter "applicable strip thickness".
[0021] In Table 1, the welding machine speed refers to the speed at which the welding wheel travels.
[0022] In Table 1, welding pressure refers to the pressure exerted by the welding wheel on the surface of the strip through the cylinder lifting and lowering.
[0023] In Table 1, the "weld width" is determined by the width of the upper electrode welding wheel. When switching processes, the welding wheel should be replaced or welding wheels of different sizes should be set on the welding machine.
[0024] 2. Electrode selection: The lower electrode of the present invention is a plate electrode, and the strip is laid on the electrode after overlapping. The upper electrode is a wheel electrode, which rolls on the surface of the strip. The electrode material is beryllium copper, and the performance of the selected beryllium copper material after heat treatment should meet the following standards.
[0025]
[0026] A circulating cooling water channel is set inside the welding wheel and the plate electrode to reduce the high temperature generated by welding and protect the electrode itself from deformation or loss of lubricating oil due to high temperature.
[0027] Clean the strip surface before welding. The standard is: the residual oil on one side is less than 300mg / m 2 , the iron powder residue on one side is less than 100 mg / m 2 .
[0028] Figure 1 The figure is a schematic diagram of precision resistance welding of iron-chromium-aluminum strips. After the surface of strip 1 and strip 2 is cleaned, the head and tail are overlapped together and placed on the lower electrode 5. The two ends are aligned, and the upper electrode is pressed down by the cylinder and a certain pressure is maintained during the welding process. After the welding is started, the welding wheel moves on the surface of the strip at a certain welding speed, and direct current is passed between the upper electrode and the lower electrode. Under the action of high current, the temperature of the contact part of the weld seam rises rapidly to above the melting point, so that the material melts and forms a molten core. The moving speed of the welding wheel is controlled by a variable frequency motor, and the pressure pressed by the welding wheel is controlled by a gas pressure reducing valve. In order to protect the electrode from damage under frequent welding, cooling water 2 is circulated inside the electrode to ensure that the electrode is at a reasonable temperature. The weld width of the welding is determined by the width of the arc surface of the welding wheel. If the weld width parameter needs to be changed, the welding wheel should be replaced. At the same time, in order to ensure the accuracy of the welding process, the welding wheel should be regularly repaired to ensure that the welding wheel width is controlled within the target range.
[0029] The welding method provided by the present invention includes the welding process and the selection of welding electrode materials. Different welding processes should be selected for precision iron-chromium-aluminum alloy strips of different specifications.
[0030] Definition 1: In this article, the term iron-chromium-aluminum alloy refers to the iron-chromium-aluminum alloy with GB grade 0Cr21Al6.
[0031] Definition 2: In this article, the term "precision Fe-Cr-Al alloy strip" refers to strip with a thickness between 0.02mm and 0.5mm.
[0032] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Embodiment 1
[0033] In this example, the precision iron-chromium-aluminum alloy material with the grade of 0Cr21Al6 is selected. The specifications of strip 1 are: thickness 0.5mm, width 650mm; the specifications of strip 2 are: thickness 0.5mm, width 650mm. The steel strip is flat, smooth and wrinkle-free. The requirements for the finished welding product are: the weld is flat and there is no cracking after annealing.
[0034] Welding process: The welding process given according to the present invention is as follows.
[0035] 2. Electrode selection: The material of the welding wheel is C17200 beryllium copper alloy, with a hardness of HV414, a conductivity of 82%, a softening temperature of 930°C, and an outer diameter of 5mm.
[0036] The welding steps are as follows: After the surface of strip 1 and strip 2 is cleaned, the head and tail are overlapped together, placed on the lower electrode, the two ends are aligned, the upper electrode is pressed down, the welding process is input, and the electrode material and welding wheel size are confirmed to be correct before starting welding. After welding is completed, the surface quality of the weld is checked and the welding machine is returned to its position.
[0037] By using the welding method of Example 1 of the present invention, the 0Cr21Al6 precision iron-chromium-aluminum alloy strip is annealed in a vertical bright annealing furnace after two passes of welding. After annealing, the weld surface is smooth without cracking. Embodiment 2
[0038] In this example, the precision iron-chromium-aluminum alloy material with the grade of 0Cr21Al6 is selected. The specifications of strip 1 are: thickness 0.1mm, width 640mm; the specifications of strip 2 are: thickness 0.08mm, width 640mm. The steel strip is flat, smooth and wrinkle-free. The requirements for the finished welding product are: the weld is flat and there is no cracking after annealing.
[0039] Welding process: The welding process given according to the present invention is as follows.
[0040]
[0041] 2. Electrode selection: The material of the welding wheel is C17200 beryllium copper alloy, with a hardness of HV414, a conductivity of 82%, a softening temperature of 930°C, and an outer diameter of 3mm.
[0042] The welding steps are as follows: After the surface of strip 1 and strip 2 is cleaned, the head and tail are overlapped together, placed on the lower electrode, the two ends are aligned, the upper electrode is pressed down, the welding process is input, and the electrode material and welding wheel size are confirmed to be correct before starting welding. After welding is completed, the surface quality of the weld is checked and the welding machine is returned to its position.
[0043] By using the welding method of Example 2 of the present invention, the 0Cr21Al6 precision iron-chromium-aluminum alloy strip is annealed in a vertical bright annealing furnace after two passes of welding. After annealing, the weld surface is smooth without cracking.
[0044] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A precision iron-chromium-aluminum alloy strip welding method, characterized in that: It includes the following aspects: (1) Welding process: The electrode is a plate electrode. The strip is laid on the electrode after being overlapped. The upper electrode is a wheel electrode, which rolls on the surface of the strip. During welding, the welding wheel rolls from one side of the strip to the other side. During welding, three-phase AC power enters the medium frequency inverter, and after rectification, filtering and inversion, the medium frequency AC voltage is output to the medium frequency transformer, and then the medium frequency DC power is output to the welding machine electrode after step-down and rectification by the medium frequency transformer; (2) Electrode selection: The electrode material is beryllium copper. The properties of the selected beryllium copper material after heat treatment are as follows: hardness HV: 400~450, conductivity IACS: 80%~85%, softening temperature ℃: 930~950.
2. A precision iron-chromium-aluminum alloy strip welding method according to claim 1, characterized in that: The welding process parameters are: strip thickness mm: 0.02 ~ 0.03, current kA: 2 ~ 4.5, speed m / min: 8 ~ 10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.03 ~ 0.05, current kA: 3.6 ~ 6, speed m / min: 8 ~ 10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.05 ~ 0.1, current kA: 4.5 ~ 9, speed m / min: 8 ~ 10, pressure bar: 4, weld width mm: 3; strip thickness mm: 0.1 ~ 0.25, current kA: 7.2 ~ 18, speed m / min: 6 ~ 8, pressure bar: 5, weld width mm: 5; strip thickness mm: 0.25 ~ 0.5, current kA: 15 ~ 30, speed m / min: 6 ~ 8. Pressure bar: 5, weld width mm: 5; Strip thickness refers to the thickness of the single piece of the overlapping part of the head and tail of the strip, and the welding machine speed refers to the speed of the welding wheel. The welding pressure refers to the pressure of the welding wheel on the surface of the strip through the cylinder lifting and lowering. The weld width is determined by the width of the upper electrode welding wheel. The thickness difference between the two strips welded together should not exceed 30% of the total thickness.
3. A precision iron-chromium-aluminum alloy strip welding method according to claim 1, characterized in that: A circulating cooling water channel is arranged inside the welding wheel and the plate electrode to reduce the high temperature generated by welding.
4. A precision iron-chromium-aluminum alloy strip welding method according to claim 1, characterized in that: Clean the strip surface before welding. The standard is: the residual oil on one side is less than 300mg / m 2 , the iron powder residue on one side is less than 100 mg / m 2 .