Flexible piezoresistive pressure sensor based on double-layer Janus film and preparation method thereof
By using a double-layer Janus film structure and electrospinning technology in the flexible pressure sensor, the problem of small detection range is solved, and a flexible pressure sensor with high sensitivity and wide range is realized, which is suitable for human body and larger pressure detection applications.
Patent Information
- Application Number
- CN202410975754.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-18
AI Technical Summary
The existing flexible pressure sensors have a small detection range and cannot meet the needs of large range and high sensitivity, which limits their expansion in the detection of daily physiological signals and large pressure of the human body.
A flexible piezoresistive pressure sensor based on a double-layer Janus film is used. The interdigital electrode, barrier layer, first Janus conductive layer, spacer layer and second Janus conductive layer are stacked in sequence, and a cone structure is set on the surface of the conductive layer. The MWCNT/Mxene/TPU/PVP composite layer is prepared by electrospinning and ultrasonic cavitation technology to increase the specific surface area and sensitivity of the conductive layer.
The sensitivity and measuring range of the sensor are significantly improved, and the initial current can be reduced under the action of a small force, and the resistance is increased through the double conductive layer in parallel when the pressure increases, thereby expanding the detection range.
Smart Images

Figure CN118794577A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of flexible pressure detection and flexible wearable electronic devices, and in particular to a flexible piezoresistive pressure sensor based on a double-layer Janus film and a preparation method thereof. Background Art
[0002] Pressure detection range and sensitivity are important indicators for evaluating the performance of flexible pressure sensors. Generally speaking, due to the nature of flexible materials, the range of flexible pressure sensors is small, and the larger the pressure range, the lower the sensitivity; the higher the sensitivity, the smaller the range. Many high-sensitivity flexible pressure sensors have a range within 50kPa, which cannot meet the monitoring of daily physiological signals of the human body, limiting the further development and application of flexible pressure sensors. Therefore, improving the range and sensitivity of flexible pressure sensors at the same time is of great value to expand the application of flexible pressure sensors.
[0003] However, the current detection range of flexible pressure sensors is within 700 kPa, and the sensitivity of large-range sensors is concentrated in 10 kPa. -1 Within this range, the application environment is mostly concentrated on the detection of pressure signals such as human pulse, which cannot meet the needs of larger pressure detection applications such as handling robots. Summary of the invention
[0004] The purpose of the present invention is to provide a flexible piezoresistive pressure sensor based on a double-layer Janus film and a preparation method thereof, so as to overcome the problem that the existing flexible pressure sensor has a small detection range and cannot meet the requirements of a large range and high sensitivity.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A flexible piezoresistive pressure sensor based on a double-layer Janus film comprises an interdigitated electrode, a barrier layer, a first Janus conductive layer, a spacer layer and a second Janus conductive layer which are stacked in sequence, and a cone structure is arranged on the surfaces of the barrier layer, the first Janus conductive layer, the spacer layer and the second Janus conductive layer.
[0007] Preferably, the first Janus conductive layer and the second Janus conductive layer are both made of MWCNT / Mxene / TPU / PVP composite layer.
[0008] Preferably, the height of the cone structures on the surfaces of the barrier layer, the first Janus conductive layer, the spacer layer and the second Janus conductive layer is not higher than 200 microns.
[0009] Preferably, both the barrier layer and the spacer layer are made of TPU / PVP layer.
[0010] Preferably, the thickness of the barrier layer and the spacer layer is no greater than 50 microns.
[0011] A method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film comprises the following steps:
[0012] The TPU / PVP composite film was prepared by electrospinning technology;
[0013] The MWCNT / Mxene layer was generated on the TPU / PVP composite film by ultrasonic cavitation to obtain a Janus conductive layer;
[0014] Then, an electrospinning method is used to generate a barrier layer on the interdigital electrode, and an electrospinning method is used to generate a spacer layer on one of the Janus conductive layers. Then, the interdigital electrode with the barrier layer, the Janus conductive layer with the spacer layer, and the Janus conductive layer prepared in the above steps are sequentially glued to obtain a flexible pressure sensor.
[0015] Preferably, electrospinning technology is used to generate a TPU / PVP composite film on a production template, and an electrospinning injection needle is used for silk thread output. The distance between the electrospinning injection needle and the production template is 15-25 cm, the voltage between the electrospinning injection needle and the production template is +15kV--5kV, and the injection speed of the electrospinning injection needle is 1ml / h; sandpaper is used to make the template, and the mesh number of the sandpaper is 180 mesh.
[0016] Preferably, the MWCNT / Mxene material is attached to the TPU / PVP composite film by an ultrasonic cell disruptor, the ultrasonic parameters are set to 300-400W, 30-40 minutes each time, and washed with deionized water after the ultrasonication ends. The Janus conductive layer can be obtained by cycling 2-3 times.
[0017] Preferably, a TPU / PVP composite solution is used to prepare the TPU / PVP composite film, and the TPU / PVP composite solution is prepared by mixing TPU particles, PVP powder, and DMF solution in a mass ratio of 1.3:0.14:4.
[0018] Preferably, a MWCNT / Mxene layer is formed on the TPU / PVP composite film using a MWCNT / Mxene solution, wherein the MWCNT / Mxene solution comprises a MWCNT solution and a Mxene solution in a ratio of 1:1 by weight.
[0019] Compared with the prior art, the present invention has the following beneficial technical effects:
[0020] The present invention provides a flexible piezoresistive pressure sensor based on a double-layer Janus film, comprising a finger electrode, a barrier layer, a first Janus conductive layer, a spacer layer and a second Janus conductive layer which are sequentially stacked, wherein the surfaces of the barrier layer, the first Janus conductive layer, the spacer layer and the second Janus conductive layer are all provided with a cone structure, and the sensitivity of the sensor can be greatly improved by providing the cone structure. Under the action of a relatively small force, the first Janus conductive layer of the lower layer of the double-layer conductive layer structure first contacts the finger electrode, and as the pressure continues to increase, the first Janus conductive layer and the second Janus conductive layer begin to contact, and the second Janus conductive layer also begins to conduct, and the resistance of the entire pressure-sensitive layer changes from the contact resistance of a single conductive layer and the finger electrode to the parallel connection between the double-layer conductive layers and the lower conductive layer and the finger electrode, thereby increasing the measuring range.
[0021] The present invention generates a barrier layer and a spacer layer between the interdigitated electrode and the double-layer conductive unit by electrospinning, which can effectively reduce the initial current. The rich micro-cone structure on the surface of the conductive unit can greatly improve the sensitivity of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the structure of a highly sensitive, wide-range flexible piezoresistive pressure sensor based on a double-layer Janus film in an embodiment of the present invention.
[0023] Figure 2 Schematic diagram of the electrospinning process in an embodiment of the present invention.
[0024] In the figure, 1, interdigitated electrode; 2, barrier layer; 3, first Janus conductive layer; 4, spacer layer 4; 5, second Janus conductive layer 5. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0026] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0027] like Figure 1 As shown, the present invention provides a high-sensitivity wide-range flexible piezoresistive pressure sensor based on a double-layer Janus film, comprising a finger electrode 1, a barrier layer 2, a first Janus conductive layer 3, a spacer layer 4, and a second Janus conductive layer 5 which are sequentially stacked. In the present application, a double-layer conductive layer in which the first Janus conductive layer 3 and the second Janus conductive layer 5 are spaced apart is used as a pressure-sensitive layer, which can effectively reduce the initial current. The rich micro-cone structures on the surfaces of the first Janus conductive layer 3 and the second Janus conductive layer 5 can greatly improve the sensitivity of the sensor. Under the action of a small force, the first Janus conductive layer 3 of the lower layer of the double-layer conductive layer structure first contacts the finger electrode. As the pressure continues to increase, the first Janus conductive layer 3 and the second Janus conductive layer 5 begin to contact, and the second Janus conductive layer 5 also begins to conduct. The resistance of the entire pressure-sensitive layer changes from the contact resistance of a single conductive layer and the finger electrode to the parallel connection between the double-layer conductive layers and the lower conductive layer and the finger electrode, thereby increasing the range.
[0028] In a specific embodiment of the present application, the interdigitating electrode 1 is disposed on a substrate, and the substrate serves as a receiving structure for the interdigitating electrode 1 .
[0029] In a specific embodiment of the present application, the first Janus conductive layer and the second Janus conductive layer both use a two-dimensional material carbon nanotube / titanium carbide / polyvinyl alcohol / polyvinyl pyrrolidone (MWCNT / Mxene / TPU / PVP) composite layer. Specifically, a two-dimensional material carbon nanotube / titanium carbide / polyvinyl alcohol / polyvinyl pyrrolidone (MWCNT / Mxene / TPU / PVP) composite material is used as the conductive material to prepare the MWCNT / Mxene / TPU / PVP composite layer, i.e., the first Janus conductive layer and the second Janus conductive layer.
[0030] A plurality of micro-cone structures are arranged on the surfaces of the first Janus conductive layer and the second Janus conductive layer to increase the specific surface area of the first Janus conductive layer and the second Janus conductive layer, and the height of the micro-cone structure is not higher than 200 microns.
[0031] In a specific embodiment of the present application, both the barrier layer 2 and the spacer layer 4 are made of polyvinyl alcohol / polyvinyl pyrrolidone (TPU / PVP) layers.
[0032] The surface arrays of the barrier layer 2 and the spacer layer 4 have multiple micro-cone structures, and the height of the micro-cone structures is not higher than 200 microns. Specifically, according to the thickness requirements of the barrier layer 2 and the spacer layer 4, the barrier layer 2 and the spacer layer 4 adopt an ultra-thin structure; the thickness of the barrier layer 2 and the spacer layer 4 is not more than 50 microns.
[0033] In another embodiment of the present invention, a method for preparing a high-sensitivity, wide-range flexible piezoresistive pressure sensor of a double-layer Janus film is provided, which specifically comprises the following steps:
[0034] The TPU / PVP composite film was prepared by electrospinning technology;
[0035] The MWCNT / Mxene layer was generated on the TPU / PVP composite film by ultrasonic cavitation to obtain a Janus conductive layer;
[0036] Then, an electrostatic spinning method is used to generate a barrier layer on the finger electrode, and an electrostatic spinning method is used to generate a spacer layer on one of the Janus conductive layers, and then the finger electrode with the barrier layer, the Janus conductive layer with the spacer layer, and the Janus conductive layer prepared by the above steps are sequentially glued to obtain a flexible pressure sensor. The present invention generates a barrier layer and a spacer layer between the finger electrode and the double-layer conductive unit by electrostatic spinning, which can effectively reduce the initial current. The rich micro-cone structure on the surface of the conductive unit can greatly improve the sensitivity of the sensor. Under the action of a small force, the lower conductive unit of the double-layer conductive unit structure first contacts the finger electrode. As the pressure continues to increase, the upper layer begins to contact the lower layer, and the upper conductive unit also begins to conduct. The resistance of the entire conductive unit changes from the contact resistance of a single conductive unit and the finger electrode to the parallel connection between the double-layer conductive layers and the lower conductive layer and the finger electrode, thereby increasing the range.
[0037] The electrospinning technology is used to prepare a TPU / PVP composite film, and sandpaper is used as a production template; the mesh number of the sandpaper is 180 meshes, and the electrospinning technology is used to generate the TPU / PVP composite film on the production template; specifically, in the process of generating the TPU / PVP composite film on the production template by the electrospinning technology, the production template is set as a rotating body, and an electrospinning injection needle is used for silk thread output, the distance between the electrospinning injection needle and the production template is 15-25cm, the voltage between the electrospinning injection needle and the production template is +15kV--5kV, the injection speed of the electrospinning injection needle is 1ml / h, and the production template is rotated for 2h to obtain the TPU / PVP composite film for preparing the Janus conductive layer.
[0038] The ultrasonic cavitation method is used to attach the MWCNT / Mxene material to the TPU / PVP composite film; specifically, the MWCNT / Mxene material is attached to the TPU / PVP composite film by an ultrasonic cell disruptor, the ultrasonic parameters are set to 300-400W, each time for 30-40 minutes, and after the ultrasound is finished, it is washed with deionized water, and the cycle is repeated 2-3 times to obtain the Janus conductive layer.
[0039] In the process of preparing the Janus conductive layer, sandpaper is used as a template, with one side convex and the other side concave. After ultrasonic cavitation, the MWCNT / Mxene material will cover the convex surface to increase the specific surface area. On the other side, due to the concave surface, more MWCNT / Mxene material will be deposited in the concave area, which has stronger conductivity, and the two sides constitute a Janus conductive film.
[0040] When the TPU / PVP film prepared by electrospinning of the present invention is subjected to ultrasonic cavitation, wrinkles appear on the surface of the fibers constituting the film because the PVP material is easily soluble in water, thereby increasing the specific surface area of the fibers, absorbing more MWCNT / Mxene materials, and increasing the conductivity of the film.
[0041] A barrier layer and a spacer layer are generated on the interdigitated electrode 1 and the Janus conductive layer, respectively, and an electrospinning injection needle is used for silk thread output. The distance between the electrospinning injection needle and the production template is 15-25 cm, the voltage between the electrospinning injection needle and the production template is +15kV--5kV, the injection speed of the electrospinning injection needle is 1ml / h, and the production template rotation spinning time is 10min, and a TPU / PVP composite film can be obtained for use as a barrier layer 2 and a spacer layer 4.
[0042] In a specific embodiment of the present application, the preparation of the TPU / PVP composite film is firstly to prepare a TPU / PVP composite solution, and take TPU particles, PVP powder and DMF solution respectively in a mass ratio of 1.3:0.14:4, and fully dissolve the TPU particles and PVP powder in the DMF solution; specifically, the TPU particles and PVP powder are stirred in the DMF solution with a magnetic stirrer, the speed is set to 300r / min, the temperature is 80°C, and the TPU / PVP solution is prepared after stirring for 3 hours.
[0043] like Figure 2 As shown, the TPU / PVP solution is poured into a syringe, and then the injection speed is set to 1 ml / h, the electrospinning voltage is set to +15V, -5V, the distance between the needle and the receiver is 20 cm, the receiver drum speed is set to 200 r / min, the spinning time is set to 10min-2h, the spinning temperature is controlled at 30°C, the humidity is controlled at 30-40% RH, and 180 mesh sandpaper and finger electrodes are placed on the receiver, respectively, to obtain a TPU / PVP composite film with a micro-cone structure and an ultra-thin TPU / PVP spacer layer and a TPU / PVP barrier layer; in this application, the barrier layer and the spacer layer are the same.
[0044] Example
[0045] MWCNT / Mxene / TPU / PVP conductive film and sensor preparation:
[0046] Preparation of Mxene solution:
[0047] Ti3C2Tx was synthesized by etching the Ti3AlC2Max phase with LiF / HCl solution.
[0048] First, 3.2 g LiF and 40 ml 9 M HCl were added to the reactor, and then the reactor was placed in a constant temperature water bath, set to 40 ° C, and stirred for 15 minutes. Then 2 g Ti3AlC2 was added to the reactor and then reacted for 48 hours. The obtained acidic suspension was washed with deionized water and centrifuged repeatedly until the solution was neutral. The resulting precipitate was collected and dispersed in deionized water, and then ultrasonically treated under Ar bubbling for 40 minutes; finally, the MXene suspension was centrifuged at 3500 rpm for 1 hour to obtain a uniform few-layer MXene solution.
[0049] MWCNT / Mxene solution;
[0050] First, 10 mg of MWCNT powder was weighed and placed in 10 ml of water, and ultrasonic dispersion was performed to uniformly disperse it to form a MWCNT aqueous dispersion with a concentration of 1 mg / ml. The MXene suspension prepared above was diluted to 5 mg / ml, 10 ml was taken out with a pipette, mixed with the 10 ml MWCNT aqueous dispersion prepared above, and ultrasonic treatment was performed for 2 hours to uniformly disperse it to form a MWCNT / MXene solution.
[0051] Preparation of MWCNT / Mxene / TPU / PVP film:
[0052] The prepared micro-cone TPU / PVP film is placed in the prepared 5mg / ml Mxene solution, and then ultrasonicated in an ultrasonic cell disruptor. The Mxene nanosheets are embedded in the TPU / PVP fibers through ultrasonic cavitation. The ultrasonic power is set to 300-400W, and the ultrasonic time is set to 30-40mins. During the ultrasonic process, the solution temperature is kept below 40°C to avoid Mxene oxidation during the ultrasonic process. After the ultrasonic process, the film is placed in deionized water to wash the surface. Repeat the whole process 2-3 times to obtain a uniform MWCNT / Mxene / TPU / PVP film. The film is then placed in a vacuum drying oven for drying, and the drying temperature is set to 50°C for 1h. Subsequently, a MWCNT / Mxene / TPU / PVP conductive film with a purple-black surface is obtained.
[0053] Sensor preparation
[0054] The obtained MWCNT / Mxene / TPU / PVP film was then spun in the above-mentioned electrospinning device for 10 minutes to obtain an ultra-thin spacer layer. The interdigitated electrode, ultra-thin TPU / PVP spacer layer, MWCNT / Mxene / TPU / PVP conductive film, ultra-thin TPU / PVP spacer layer, and MWCNT / Mxene / TPU / PVP conductive film structure were assembled using double-sided tape, and the sensor was packaged using polyimide to obtain a flexible pressure sensor.
Claims
1. A flexible piezoresistive pressure sensor based on a double-layer Janus film, characterized in that: The invention comprises an interdigitated electrode (1), a barrier layer (2), a first Janus conductive layer (3), a spacer layer (4) and a second Janus conductive layer (5) which are sequentially stacked, and the surfaces of the barrier layer (2), the first Janus conductive layer (3), the spacer layer (4) and the second Janus conductive layer (5) are all provided with a cone structure.
2. The flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 1, characterized in that: The first Janus conductive layer and the second Janus conductive layer both use MWCNT / Mxene / TPU / PVP composite layers.
3. The flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 1, characterized in that: The height of the cone structures on the surfaces of the barrier layer (2), the first Janus conductive layer (3), the spacer layer (4) and the second Janus conductive layer (5) is no greater than 200 micrometers.
4. The flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 1, characterized in that: The barrier layer (2) and the spacer layer (4) are both made of TPU / PVP layers.
5. The flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 1, characterized in that: The thickness of the barrier layer (2) and the spacer layer (4) is no more than 50 microns.
6. A method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film, characterized in that: The following steps are involved: The TPU / PVP composite film was prepared by electrospinning technology; The MWCNT / Mxene layer was generated on the TPU / PVP composite film by ultrasonic cavitation to obtain a Janus conductive layer; Then, an electrospinning method is used to generate a barrier layer on the interdigital electrode, and an electrospinning method is used to generate a spacer layer on one of the Janus conductive layers. Then, the interdigital electrode with the barrier layer, the Janus conductive layer with the spacer layer, and the Janus conductive layer prepared in the above steps are sequentially glued to obtain a flexible pressure sensor.
7. The method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 6, characterized in that: Electrospinning technology is used to generate TPU / PVP composite film on the production template, and an electrospinning injection needle is used for silk thread output. The distance between the electrospinning injection needle and the production template is 15-25 cm, the voltage between the electrospinning injection needle and the production template is +15kV~-5kV, and the injection speed of the electrospinning injection needle is 1ml / h; sandpaper is used to make the template, and the mesh number of the sandpaper is 180 mesh.
8. The method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 6, characterized in that: The MWCNT / Mxene material is attached to the TPU / PVP composite film by an ultrasonic cell disruptor, the ultrasonic parameters are set to 300-400W, 30-40 minutes each time, and washed with deionized water after the ultrasonication. After 2-3 cycles, the Janus conductive layer can be obtained.
9. The method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 6, characterized in that: The TPU / PVP composite film is prepared by using a TPU / PVP composite solution, which is prepared by mixing TPU particles, PVP powder and DMF solution in a mass ratio of 1.3:0.14:
4.
10. The method for preparing a flexible piezoresistive pressure sensor based on a double-layer Janus film according to claim 6, characterized in that: A MWCNT / Mxene solution is used to form a MWCNT / Mxene layer on a TPU / PVP composite film. The MWCNT / Mxene solution includes a MWCNT solution and a Mxene solution in a mass ratio of 1:1.