A low-cost solar cell electrode and preparation method thereof

By using copper mirror reaction liquid in HJT solar cells to form copper seed layer and combining copper plating technology, the high cost and copper migration problems are solved, and efficient and low-cost solar cell electrode preparation is achieved, and the battery conversion efficiency is improved.

CN118800842BActive Publication Date: 2024-11-26SHENZHEN APG MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411281449.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing HJT solar cell metal gate wire electrode preparation method is costly and copper is easily migrated to the TCO layer during copper plating, affecting the photoelectric conversion efficiency of the battery.

Method used

The copper seed layer is formed in the copper mirror reaction using copper mirror reaction, and the adhesion is enhanced through annealing treatment. The copper plating layer is prepared in combination with the copper electroplating process. Finally, the excess copper seed layer is removed, and the copper seed layer is prepared instead of PVD equipment, which reduces the cost and Improve uniformity and adhesion of copper seed layer.

Benefits of technology

A low-cost solar cell electrode preparation is achieved, and the copper seed layer is uniformly distributed, which prevents electroplating defects, improves battery conversion efficiency, reduces labor costs, and avoids the reduction in photoelectric conversion efficiency caused by copper migration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800842B_ABST
    Figure CN118800842B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of solar cells, and provides a low-cost solar cell electrode and a preparation method thereof, including: providing a solar cell precursor to be metallized; performing a graphic treatment on the solar cell precursor to form a grid line pattern; placing the solar cell precursor containing the grid line pattern in a copper mirror reaction solution for reduction reaction, and then annealing to form a copper seed layer; using a copper electroplating process to prepare a copper coating on the surface of the copper seed layer, and then removing the mask layer outside the grid line pattern and the copper seed layer on the mask layer to form a solar cell electrode. The preparation method provided in the present application can replace PVD equipment to prepare a copper seed layer, without the need to use expensive equipment, and at a low cost. In addition, the present application uses a copper mirror reaction to enable copper to be uniformly deposited on the bottom and side walls of the grid line pattern groove, so that the copper seed layer is more evenly distributed, thereby preventing defects from forming during the electroplating process, and facilitating subsequent electroplating to form a uniform and dense copper coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of solar cells, and in particular to a low-cost solar cell electrode and a preparation method thereof. Background Art

[0002] Amorphous silicon / crystalline silicon heterojunction (HJT) solar cells have the advantages of high conversion efficiency, low process temperature, and high stability, and have become the focus of current research in the field of solar cells. The metal grid electrodes of current HJT solar cells are generally formed by screen-printing low-temperature silver paste, which is then sintered and solidified. However, the precious metal silver in the low-temperature silver paste generally accounts for about 90% of the silver paste, resulting in excessively high battery production costs, and the width and aspect ratio of the silver grid lines are limited by the screen printing process, which hinders further improvement of battery efficiency. Therefore, in order to reduce costs and increase efficiency of HJT solar cells, the industry has introduced a technical route for electroplating copper grid lines to replace traditional screen-printed low-temperature silver paste.

[0003] The electroplating of copper grid lines includes the preparation of copper seed layer, patterning, copper electroplating and post-processing. Among them, the preparation of copper seed layer is crucial. It plays a conductive role in the copper electroplating process, allowing the electroplating process to proceed smoothly, and at the same time enhances the adhesion between the electroplated copper layer and TCO to prevent falling off. At present, PVD (Physical Vapor Deposition) equipment is mainly used to deposit copper seed layer on the TCO (transparent conductive oxide) film of silicon wafer in the whole area. However, PVD equipment is expensive, and in the post-processing stage, after removing the mask layer, the excess copper seed layer must be removed to complete the metallization process. The process is complicated and the labor cost is too high, so it is difficult to achieve the purpose of reducing costs and increasing efficiency. In addition, during the copper electroplating process, the copper in the copper seed layer is easy to migrate to the TCO layer and affect the light transmittance of the TCO layer, and even diffuse to the silicon body to cause silicon body contamination, which will eventually affect the photoelectric conversion efficiency of solar cells. Summary of the invention

[0004] The purpose of the present application is to provide a low-cost solar cell electrode and a method for preparing the same, in order to solve the problems of high cost in the existing method for preparing solar cell electrodes, and the problem that copper easily migrates to the TCO layer during copper electroplating, and even diffuses into the silicon body, thereby affecting the photoelectric conversion efficiency of the cell.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present application provides a low-cost method for preparing a solar cell electrode, comprising the following steps:

[0007] providing a solar cell precursor to be metallized;

[0008] Performing a patterning process on the solar cell precursor to form a grid line pattern;

[0009] Placing the solar cell precursor containing the grid line pattern in a copper mirror reaction solution for reduction reaction, and then annealing to form a copper seed layer;

[0010] A copper plating layer is prepared on the surface of the copper seed layer by using a copper electroplating process, and then the mask layer outside the grid line pattern and the copper seed layer on the mask layer are removed to form a solar cell electrode.

[0011] In a second aspect, the present application provides a low-cost solar cell electrode, including a solar cell electrode prepared by the preparation method provided in the present application.

[0012] Compared with the prior art, this application has the following beneficial effects:

[0013] (1) The solar cell precursor to be metallized is first patterned to form a grid line pattern, then placed in a copper mirror reaction solution for a reduction reaction to form a copper seed layer, and then electroplated to form a copper plating layer. Finally, the mask layer outside the grid line pattern and the copper seed layer attached to the mask layer are removed to form an electrode. Therefore, it can replace PVD equipment to prepare the copper seed layer, and there is no need to use expensive equipment, which is lower in cost.

[0014] (2) Compared with the PVD method, the copper mirror reaction used in the present application can make copper evenly deposited on the bottom and side walls of the gate line pattern groove, making the copper seed layer more evenly distributed, thereby preventing defects from forming during the electroplating process and facilitating the subsequent electroplating to form a uniform and dense copper plating layer.

[0015] (3) The copper seed layer and copper plating layer of the present application are embedded in the TCO layer, which has better contact with the TCO layer, smaller contact resistance, and can prevent falling off, which is beneficial to improving the battery conversion efficiency.

[0016] (4) The present application first forms a local copper seed layer by patterning, which can prevent the copper in the copper seed layer outside the gate line pattern from migrating to the TCO layer during the copper electroplating process and affecting the light transmittance of the TCO layer, or even diffusing into the silicon body to cause pollution. Therefore, the battery has a higher photoelectric conversion efficiency.

[0017] (5) Compared with the traditional method of first preparing a copper seed layer and then patterning it, the present invention has a simpler process for removing the excess copper seed layer on the mask layer and has lower labor costs due to the poor adhesion between the mask layer and the copper seed layer on the mask layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0019] Figure 1 is a process flow chart of a low-cost method for preparing a solar cell electrode provided in an embodiment of the present application;

[0020] Figure 2 It is a schematic diagram of the structure of a solar cell electrode prepared by the low-cost method for preparing a solar cell electrode provided in an embodiment of the present application. DETAILED DESCRIPTION

[0021] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0022] The first aspect of the present application provides a low-cost method for preparing a solar cell electrode, such as Figure 1 As shown, the following steps are included:

[0023] S01: providing a solar cell precursor to be metallized;

[0024] S02: The solar cell precursor is patterned to form a grid line pattern (such as Figure 1 as shown in D);

[0025] S03: placing the solar cell precursor containing the grid line pattern in a copper mirror reaction solution for reduction reaction, and then annealing to form a copper seed layer (such as Figure 1 D and E);

[0026] S04: Prepare a copper plating layer on the surface of the copper seed layer using a copper electroplating process (such as Figure 1 Then, the mask layer outside the gate line pattern and the copper seed layer on the mask layer are removed to form a solar cell electrode (as shown in F). Figure 1 H).

[0027] The low-cost method for preparing solar cell electrodes provided in the embodiment of the present application is to firstly perform a patterning process on the solar cell precursor to be metallized to form a grid line pattern, then place it in a copper mirror reaction solution for a reduction reaction to form a copper seed layer, then perform electroplating to thicken it to form a copper plating layer, and finally remove the mask layer outside the grid line pattern and the copper seed layer attached to the mask layer to form an electrode. Therefore, it can replace the PVD equipment to prepare the copper seed layer, without the need to use expensive equipment, and the cost is lower. In addition, due to the poor adhesion between the mask layer and the copper seed layer on the mask layer, compared with the traditional process of first preparing the copper seed layer and then patterning it, the process of removing the mask layer outside the grid line pattern and the excess copper seed layer on the mask layer in the present application is simpler and has lower labor costs. In addition, compared to the copper seed layer prepared by PVD equipment, the copper mirror reaction used in this application can make copper evenly deposited on the bottom and side walls of the grid line pattern groove, making the copper seed layer more evenly distributed, thereby preventing defects from forming during the electroplating process, and facilitating the subsequent electroplating to form a uniform and dense copper plating layer. At the same time, the copper seed layer and copper plating layer of this application are embedded in the TCO layer, which has better contact with the TCO layer, has a smaller contact resistance, and can also prevent falling off, so it is beneficial to improve the battery conversion efficiency. In addition, this application first graphically forms a local copper seed layer to prevent the copper in the copper seed layer outside the grid line pattern from migrating to the TCO layer during the copper electroplating process and affecting the light transmittance of the TCO layer, or even diffusing to the silicon body to cause pollution, so the battery has a higher photoelectric conversion efficiency.

[0028] In the above step S01, the solar cell precursor to be metallized may refer to a solar cell precursor that has not yet prepared a metal grid electrode. Taking a silicon heterojunction (HJT) solar cell as an example, the solar cell precursor to be metallized may include an n-type single crystal silicon wafer substrate, an intrinsic amorphous silicon film (ia-Si:H) and a p-type amorphous silicon film (pa-Si:H) sequentially stacked on the front of the n-type single crystal silicon wafer substrate, an intrinsic amorphous silicon film (ia-Si:H) and an n-type amorphous silicon film (na-Si:H) sequentially stacked on the back of the n-type single crystal silicon wafer substrate, and a TCO film deposited on the p-type amorphous silicon film and the n-type amorphous silicon film, respectively.

[0029] In the above step S02, the step of patterning the solar cell precursor includes: preparing a mask layer (such as Figure 1 Then, the TCO layer outside the mask layer is etched to form a gate line pattern (as shown in A and B in FIG. Figure 1 Specifically, the step of preparing a mask layer on the surface of the TCO layer of the solar cell precursor includes: coating a photoresist on the surface of the TCO layer of the solar cell precursor, performing an exposure treatment after drying, and then removing the photoresist in the exposed area in a developer to form a mask layer on the surface of the TCO layer.

[0030] In the above step S03, the copper mirror reaction solution includes a copper source, a manganese source, a reducing agent and an additive in a molar ratio of 1 / (0.01-0.08) / (1.2-1.5) / (1.1-1.4). 2+ , the manganese source provides Mn 2+ , these Mn 2+ and Cu 2+ Under the action of the reducing agent, it can be reduced to form a manganese-doped copper seed layer. The additive can prevent Mn 2+ and Cu 2+ The formation of precipitation promotes the 2+ and Cu 2+ The reduction results in a smooth and dense manganese-doped copper seed layer, thereby helping to reduce the contact resistance with the TCO layer.

[0031] In an embodiment, the copper mirror reaction solution further comprises a silver source; wherein the molar ratio of the copper source, the manganese source, the silver source, the reducing agent and the additive is 1 / (0.01-0.08) / (0.01-0.05) / (1.2-1.5) / (1.1-1.4). The silver source provides Ag + , these Ag + With Mn 2 + , Cu 2+ Under the action of a reducing agent, the copper seed layer doped with manganese and silver can be reduced to form.

[0032] In an embodiment, the step of placing a solar cell precursor containing a grid line pattern in a copper mirror reaction solution comprises: placing the solar cell precursor containing a grid line pattern in a mixed solution containing a copper source, a manganese source, a silver source and an additive, and then adding a reducing agent for stirring. The temperature of the reduction reaction is 40-50°C, the pH value is 8-9.5, and the time is 5-20 minutes. The reaction conditions are mild, which can avoid corrosion of the silicon-based substrate and the amorphous silicon film and affect the battery conversion efficiency.

[0033] In the embodiment, the annealing treatment is performed in a vacuum or reducing atmosphere, at a temperature of 200-300° C., for a time of 1-4 hours. The annealing condition can not only prevent the oxidation of the copper seed layer, but also enhance the adhesion between the copper seed layer and the TCO layer, and prevent the copper seed layer from falling off; in addition, by heating, the Ag and Mn doped in the copper seed layer obtain sufficient energy, and at the same time, driven by defects, vacancies or chemical potential differences at the interface between the TCO layer and the copper seed layer, the Ag and Mn atoms tend to migrate to the interface position with lower energy, and there may also be a strong chemical interaction between Mn and the oxygen element in the TCO layer, which is conducive to promoting the migration of Mn atoms to the interface. Therefore, after annealing, the Ag and Mn doped in the copper seed layer will migrate to the interface of the TCO layer to enrich and form a silver-manganese barrier layer, so that manganese can block the subsequent copper electroplating thickening process, and the migration of copper to the TCO layer during the use of the solar cell to affect the light transmittance of the TCO layer, and prevent diffusion to the silicon body to cause silicon body pollution, so the battery has a higher photoelectric conversion efficiency, and Ag can reduce the contact resistance between the TCO layer and the copper metal electrode layer, which is beneficial to the transmission of carriers.

[0034] In an embodiment, the copper source is selected from at least one of copper sulfate, copper chloride and copper nitrate.

[0035] In an embodiment, the manganese source is selected from at least one of manganese sulfate, manganese chloride and manganese nitrate.

[0036] In an embodiment, the silver source is selected from at least one of silver nitrate, silver chloride and silver acetate.

[0037] In an embodiment, the reducing agent is selected from at least one of dimethylamine borane, hydrazine hydrate, and hypophosphite, which can reduce Sn to 2+ 、Ag + and Cu 2+ Reduction, avoid using strong alkali such as sodium hydroxide to corrode the silicon-based substrate and amorphous silicon film and affect the battery conversion efficiency.

[0038] In an embodiment, the additive includes disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol, and thiourea in a molar ratio of (1.06-1.25) / (0.005-0.02) / (0.02-0.06) / (0.005-0.02) / (0.01-0.05). 2+ Formation of complexes to prevent Cu 2+ The formation of hydroxide precipitates facilitates the Cu 2+The invention discloses a novel method for reducing the copper mirror reaction liquid to form a copper seed layer; polyethyleneimine can promote the uniformity and density of the copper seed layer, reduce the surface roughness of the copper seed layer, and enhance the conductivity; ethylene oxide can reduce the surface tension of the liquid, make the plating solution in close contact with the surface of the substrate, and improve the adhesion, surface smoothness and brightness of the copper seed layer; polyethylene glycol has the effect of leveling and fine crystallization of the copper seed layer; thiourea can reduce the formation of Cu2O, improve the stability of the copper mirror reaction liquid, and at the same time has strong adsorption, and promotes the reduction of copper ions at a low concentration, thereby increasing the plating speed. Therefore, under the compounding of the specific contents of these additives, there is a synergistic effect, so that the obtained copper seed layer is more uniform, dense, smooth and has stronger adhesion.

[0039] In an embodiment, the thickness of the copper seed layer is 100-300 nm.

[0040] In the above step S04, the step of preparing a copper plating layer on the surface of the copper seed layer by using a copper electroplating process includes: adding an electroplating solution into a plating tank, using a phosphor copper plate as an anode and a solar cell precursor containing a copper seed layer as a cathode, respectively connected to the positive and negative electrodes of a power source, and then at a temperature of 20-25°C and a current density of 2-6A / dm 2 Electroplating is carried out for 0.5~2h under the conditions of 2+ Entering the plating solution, the Cu in the plating solution 2+ The copper seed layer of the solar cell precursor is reduced to a copper coating, so after 0.5-2 hours of electroplating, a copper coating with a thickness of 5-15 μm can be obtained. Using a phosphor copper plate doped with a small amount of phosphorus as the anode can improve the stability of the plating solution, control the dissolution rate of copper, reduce the generation of anode mud and copper powder, and maintain the balance of copper ions in the plating solution.

[0041] In an embodiment, the electroplating solution includes copper sulfate, sulfuric acid, sodium chloride, a leveler, an organic additive, and water. The electroplating solution contains copper sulfate, which can keep Cu 2+ The concentration of cations remains unchanged, making the coating uniform and firm while eliminating interference from other cations.

[0042] In an embodiment, the leveler is selected from ethoxylated polyamine and / or polyvinyl pyridine. Adding these levelers can inhibit the transitional deposition of copper, thereby obtaining a uniform and dense copper plating layer.

[0043] In an embodiment, the organic additive includes polyethylene glycol (PEG 8000) and sodium polydisulfide propane sulfonate (SPS). PEG 8000 can be oriented and adsorbed at the interface between the cathode and the electroplating solution, thereby enhancing cathode polarization, inhibiting copper electrodeposition, and improving the compactness of the copper plating layer, but has no effect on improving the appearance of the copper plating layer. Since the SPS molecule contains a disulfide bond, it breaks into two sodium mercapto-1-propane sulfonate molecules under the action of an electric field, and has a depolarizing effect during the copper electrodeposition process, which can accelerate the electrodeposition. Therefore, under the synergistic effect of PEG and SPS, copper deposition can be accelerated, and the flatness and compactness of the copper plating layer can be improved.

[0044] In an embodiment, before placing the solar cell precursor containing the grid line pattern in the copper mirror reaction solution for reduction reaction, the step further includes: performing plasma treatment on the solar cell precursor containing the grid line pattern. The plasma treatment can enhance the bonding between the copper seed layer and the TCO layer, and prevent the copper seed layer and the subsequently thickened copper plating layer from falling off.

[0045] In an embodiment, before removing the mask layer outside the gate line pattern and the copper seed layer on the mask layer, the method further includes: preparing a copper-nickel alloy plating layer (such as Figure 1 G); wherein the thickness of the copper-nickel alloy plating layer is 2-5 μm; and the mass ratio of copper to nickel in the copper-nickel alloy plating layer is (6-8) / (2-4). The copper-nickel alloy plating layer covers the surface of the copper plating layer, can protect the copper plating layer from oxidation, and can improve the corrosion resistance and weldability of the solar cell electrode.

[0046] Specifically, the steps of preparing a copper-nickel alloy coating on the surface of a copper coating by an electroplating process include: adding an electroplating solution into a plating tank, using a copper-nickel alloy plate (nickel accounts for 30 wt%) as an anode, and a solar cell precursor containing a copper coating as a cathode, which are respectively connected to the positive and negative electrodes of a power source, and then at a temperature of 50-60°C and a current density of 2-5 A / dm 2 Electroplating is carried out for 10min~40min under the conditions of ; wherein the electroplating solution includes 80~100g / L nickel sulfate hexahydrate, 5~15g / L copper sulfate pentahydrate, 155~162g / L sodium citrate, 10~30g / L boric acid, 2~5g / L sodium chloride and 0~1g / L sodium dodecyl sulfate; specifically, the sodium dodecyl sulfate may be 0.2~1g / L. Since the electrode potential of copper is more positive than that of nickel, copper will precipitate preferentially. Therefore, by adding sodium citrate as a ligand in the electroplating solution, the discharge rate of copper ions is slowed down, and the precipitation of copper ions is slowed down, so that a copper-nickel alloy coating with a mass ratio of copper to nickel of (6~8) / (2~4) and a thickness of 2~5μm can be obtained through electroplating.

[0047] The second aspect of the present application provides a low-cost solar cell electrode, the specific structure of which is as follows: Figure 2 As shown, it includes a solar cell electrode prepared by the preparation method provided in the present application.

[0048] The low-cost solar cell electrode provided in the embodiment of the present application includes the solar cell electrode prepared by the preparation method provided in the present application, so the contact resistance between the electrode and the TCO layer is smaller, which is beneficial to improving the cell conversion efficiency.

[0049] The following describes the invention in conjunction with specific embodiments.

[0050] Example 1

[0051] This embodiment provides a low-cost method for preparing a solar cell electrode, comprising the following steps:

[0052] S11: providing a HJT solar cell precursor to be metallized, which includes an n-type single crystal silicon wafer, an intrinsic amorphous silicon film and a p-type amorphous silicon film sequentially stacked on the front side of the n-type single crystal silicon wafer, an intrinsic amorphous silicon film and an n-type amorphous silicon film sequentially stacked on the back side of the n-type single crystal silicon wafer, and an ITO film respectively deposited on the p-type amorphous silicon film and the n-type amorphous silicon film;

[0053] S12: coating a photoresist of brand BP218 on the surface of the TCO layer of the HJT solar cell precursor, baking at 80° C. for 8 minutes, then exposing to ultraviolet light for 60 seconds, and then placing in a developer to remove the photoresist in the exposed area, forming a mask layer on the surface of the TCO layer;

[0054] The TCO layer not covered by the mask layer is etched by a laser etcher to a depth of 100 nm to form a gate line pattern;

[0055] S13: placing a solar cell precursor containing a grid line pattern in a mixed solution of copper sulfate, manganese sulfate, silver nitrate, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea, then adding dimethylamine borane for stirring, controlling the temperature of the reaction system to 45°C and the pH to 9, and performing a reduction reaction for 10 minutes to form a manganese- and silver-doped copper seed layer (with a thickness of 105 nm), and then annealing at 250°C in vacuum for 2 hours to form a manganese-silver barrier layer at the interface of the TCO layer and the copper seed layer; wherein the molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03;

[0056] S14: Add a plating solution consisting of copper sulfate (80 g / L), sulfuric acid (230 g / L), sodium chloride (105 mg / L), ethoxylated polyamine (50 mg / L), polyethylene glycol (180 mg / L) and sodium polydisulfide propane sulfonate (2 mg / L) into the plating tank, use a phosphor copper plate as the anode, and a solar cell precursor containing a copper seed layer as the cathode, which are connected to the positive and negative electrodes of the power supply respectively, and then charge at a temperature of 22 °C and a current density of 4 A / dm 2 Electroplating was performed for 1.5 h under the conditions of , to form a copper plating layer (thickness 12.52 μm);

[0057] 90 g / L nickel sulfate hexahydrate, 10 g / L copper sulfate pentahydrate, 159 g / L sodium citrate, 25 g / L boric acid, 3 g / L sodium chloride and 0.5 g / L sodium dodecyl sulfate were added into the plating tank, a copper-nickel alloy plate (nickel accounts for 30 wt%) was used as the anode, and a solar cell precursor containing a copper coating was used as the cathode, which were connected to the positive and negative electrodes of the power supply respectively, and then the temperature was 55 ° C and the current density was 3A / dm 2 Electroplating was performed for 25 min under the conditions of , to form a copper-nickel alloy coating (thickness 3.87 μm, copper:nickel mass ratio 7 / 3);

[0058] The solar cell precursor is immersed in an acetone solution, and the mask layer outside the grid line pattern and the copper seed layer on the mask layer are removed to form a solar cell electrode.

[0059] Example 2

[0060] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0061] In step S13, the copper mirror reaction solution does not contain silver nitrate;

[0062] The molar ratio of copper sulfate, manganese sulfate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03.

[0063] Example 3

[0064] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0065] The copper mirror reaction solution does not contain disodium EDTA;

[0066] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, polyethylene imine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 0.01 / 0.04 / 0.01 / 0.03.

[0067] Example 4

[0068] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0069] The copper mirror reaction solution does not contain polyethyleneimine;

[0070] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.04 / 0.01 / 0.03.

[0071] Example 5

[0072] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0073] The copper mirror reaction solution does not contain ethylene oxide;

[0074] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.01 / 0.01 / 0.03.

[0075] Example 6

[0076] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0077] The copper mirror reaction solution does not contain polyethylene glycol;

[0078] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.01 / 0.04 / 0.03.

[0079] Example 7

[0080] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0081] The copper mirror reaction solution does not contain thiourea;

[0082] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide and polyethylene glycol is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01.

[0083] Example 8

[0084] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0085] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.01 / 0.01 / 1.2 / 1.06 / 0.02 / 0.02 / 0.02 / 0.01.

[0086] Example 9

[0087] This embodiment provides a low-cost method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0088] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.08 / 0.05 / 1.5 / 1.25 / 0.005 / 0.06 / 0.005 / 0.05.

[0089] Comparative Example 1

[0090] This comparative example provides a method for preparing a solar cell electrode, comprising the following steps:

[0091] S1: providing a HJT solar cell precursor to be metallized, which includes an n-type single crystal silicon wafer, an intrinsic amorphous silicon film and a p-type amorphous silicon film sequentially stacked on the front side of the n-type single crystal silicon wafer, an intrinsic amorphous silicon film and an n-type amorphous silicon film sequentially stacked on the back side of the n-type single crystal silicon wafer, and an ITO film respectively deposited on the p-type amorphous silicon film and the n-type amorphous silicon film;

[0092] S2: The DD-1760 series silver paste is coated on the ITO film of the HJT solar cell precursor using a screen printing process, and then sintered and cured to form a solar cell electrode.

[0093] Comparative Example 2

[0094] This comparative example provides a method for preparing a solar cell electrode, which differs from Example 1 in that:

[0095] In step S13, a copper seed layer (with a thickness of 102 nm) is prepared by using a PVD device.

[0096] Comparative Example 3

[0097] This comparative example provides a method for preparing a solar cell electrode, which differs from Example 1 in that:

[0098] In step S12, only the photoresist with brand BP218 is coated on the surface of the TCO layer of the HJT solar cell precursor, baked at 80°C for 8 minutes, and then exposed to ultraviolet light for 60 seconds. The photoresist in the exposed area is then removed in a developer to form a mask layer on the surface of the TCO layer to obtain a gate line pattern.

[0099] Comparative Example 4

[0100] This comparative example provides a method for preparing a solar cell electrode, which differs from Example 1 in that:

[0101] In step S13, the solar cell precursor containing the grid line pattern is placed in a mixed solution of copper sulfate (7.2 g / L), sodium hydroxide and sodium tartrate, and then formaldehyde (5 g / L) is added and stirred. The temperature of the reaction system is controlled to 45°C and the pH is 12. A reduction reaction is carried out for 5 minutes to form a copper seed layer (thickness of 101 nm); wherein the molar ratio of copper sulfate, sodium hydroxide, sodium tartrate and formaldehyde is 1 / 2.1 / 1.2 / 2.

[0102] Comparative Example 5

[0103] This comparative example provides a method for preparing a solar cell electrode, which differs from Example 1 in that:

[0104] The copper mirror reaction solution does not contain manganese sulfate;

[0105] The molar ratio of copper sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.03 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03.

[0106] Comparative Example 6

[0107] This comparative example provides a method for preparing a solar cell electrode, which differs from Example 1 in that:

[0108] The copper mirror reaction solution does not contain manganese sulfate and silver nitrate;

[0109] The molar ratio of copper sulfate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03.

[0110] Comparative Example 7

[0111] This embodiment provides a method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0112] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.09 / 0.06 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03.

[0113] Comparative Example 8

[0114] This embodiment provides a method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0115] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.005 / 0.005 / 1.3 / 1.2 / 0.01 / 0.04 / 0.01 / 0.03.

[0116] Comparative Example 9

[0117] This embodiment provides a method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0118] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.003 / 0.01 / 0.03 / 0.03.

[0119] Comparative Example 10

[0120] This embodiment provides a method for preparing a solar cell electrode, which is different from Embodiment 1 in that:

[0121] The molar ratio of copper sulfate, manganese sulfate, silver nitrate, dimethylamine borane, disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol and thiourea is 1 / 0.05 / 0.03 / 1.3 / 1.2 / 0.03 / 0.07 / 0.003 / 0.03.

[0122] Related performance test analysis:

[0123] 1. The solar cell electrodes prepared in Examples 1 to 9 and Comparative Examples 1 to 10 were tested for conversion efficiency (the conversion efficiency was based on Comparative Example 1, and the test value was the value increased or decreased relative to the photoelectric conversion efficiency of Comparative Example 1). The test results are shown in Table 1:

[0124] Table 1

[0125]

[0126] It can be seen from Table 1 that the battery conversion efficiency of the solar cell electrodes prepared in Examples 1 to 9 is significantly higher than the battery conversion efficiency of the solar cell electrodes prepared by screen printing silver paste in Comparative Example 1, indicating that the battery prepared by the preparation method of the solar cell electrode provided in the embodiments of the present application has a higher conversion efficiency, can replace the traditional screen printing silver paste process, and can also replace the process of preparing the copper seed layer and then electroplating thickening with PVD equipment, thereby significantly reducing the production cost of solar cells.

[0127] The cell conversion efficiency of the solar cell electrode prepared in Example 1 is significantly higher than that in Comparative Example 2, indicating that the copper mirror reaction used in the embodiment of the present application can enable copper to be evenly deposited on the bottom and side walls of the grid line pattern groove, and can make the copper seed layer more evenly distributed, which is beneficial to subsequent electroplating to form a uniform and dense copper plating layer. Therefore, the prepared copper grid line electrode is not easy to fall off, and the cell conversion efficiency is also higher.

[0128] The cell conversion efficiency of the solar cell electrode prepared in Example 1 is significantly higher than that in Comparative Example 3, indicating that the copper seed layer and the copper plating layer prepared by the preparation method provided in the embodiment of the present application are embedded in the TCO layer, and have better contact with the TCO layer and smaller contact resistance, so it is beneficial to improve the cell conversion efficiency and can also prevent falling off.

[0129] The cell conversion efficiency of the solar cell electrode prepared in Example 1 is significantly higher than that in Comparative Example 4, indicating that the present application embodiment uses dimethylamine borane as a reducing agent and can be carried out under weakly alkaline conditions. The reaction process is mild and will not cause corrosion to the silicon wafer and amorphous silicon film to affect the cell conversion efficiency. Therefore, the cell has a higher conversion efficiency.

[0130] The cell conversion efficiency of the solar cell electrode prepared in Example 1 is significantly higher than that of Comparative Examples 5 and 6. This is mainly due to the fact that the copper mirror reaction solution in the example of the present application contains a manganese source and a silver source. The manganese- and silver-doped copper seed layer forms a manganese-silver barrier layer at the interface of the TCO layer and the copper seed layer after annealing. Manganese can prevent copper from migrating to the TCO layer during the subsequent copper electroplating thickening process and affecting the light transmittance of the TCO layer, and prevent diffusion into the silicon body to cause silicon body contamination. Silver can reduce the contact resistance between the TCO layer and the copper metal electrode layer, thereby facilitating the transmission of carriers, so the battery has a higher conversion efficiency.

[0131] The cell conversion efficiency of the solar cell electrode prepared in Example 1 is significantly higher than that of Comparative Examples 7 to 10, indicating that the components of the copper mirror reaction solution are more conducive to forming a uniform, dense, smooth and more adherent copper seed layer within the specific content range of the present application, thereby reducing the contact resistance between the copper plating layer and the TCO layer, so the battery has a higher conversion efficiency.

[0132] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A low-cost method for preparing a solar cell electrode, characterized in that: The following steps are involved: providing a solar cell precursor to be metallized; Performing a patterning process on the solar cell precursor to form a grid line pattern; Placing the solar cell precursor containing the grid line pattern in a copper mirror reaction solution for reduction reaction, and then annealing to form a copper seed layer; Using a copper electroplating process to prepare a copper plating layer on the surface of the copper seed layer, and then removing the mask layer outside the gate line pattern and the copper seed layer on the mask layer to form a solar cell electrode; The copper mirror reaction solution comprises a copper source, a manganese source, a reducing agent and an additive in a molar ratio of 1 / (0.01-0.08) / (1.2-1.5) / (1.1-1.4).

2. The preparation method according to claim 1, characterized in that The copper mirror reaction solution also includes a silver source; the molar ratio of the copper source, manganese source, silver source, reducing agent and additive is 1 / (0.01-0.08) / (0.01-0.05) / (1.2-1.5) / (1.1-1.4).

3. The preparation method according to claim 2, characterized in that: At least one of the following conditions is met: The step of placing the solar cell precursor containing the grid line pattern in the copper mirror reaction solution comprises: placing the solar cell precursor containing the grid line pattern in a mixed solution containing the copper source, manganese source, silver source and additives, and then adding a reducing agent and stirring; The reduction reaction temperature is 40-50°C, the pH value is 8-9.5, and the time is 5-20 minutes; The annealing treatment is carried out in a vacuum or reducing atmosphere, at a temperature of 200-300° C., for a time of 1-4 hours.

4. The preparation method according to claim 2, characterized in that: At least one of the following conditions is met: The copper source is selected from at least one of copper sulfate, copper chloride and copper nitrate; The manganese source is selected from at least one of manganese sulfate, manganese chloride and manganese nitrate; The silver source is selected from at least one of silver nitrate, silver chloride and silver acetate; The reducing agent is selected from at least one of dimethylamine borane, hydrazine hydrate and hypophosphite; The additives include disodium ethylenediaminetetraacetate, polyethyleneimine, ethylene oxide, polyethylene glycol, and thiourea in a molar ratio of (1.06-1.25) / (0.005-0.02) / (0.02-0.06) / (0.005-0.02) / (0.01-0.05).

5. The preparation method according to claim 1, characterized in that: The step of preparing a copper plating layer on the surface of the copper seed layer by using a copper electroplating process comprises: The electroplating solution is added to the plating tank, the phosphor copper plate is used as the anode, and the solar cell precursor containing the copper seed layer is used as the cathode, which are respectively connected to the positive and negative electrodes of the power supply, and then the temperature is 20-25°C and the current density is 2-6A / dm 2 Electroplating is carried out under the conditions of 0.5~2h.

6. The preparation method according to claim 1, characterized in that: The step of patterning the solar cell precursor comprises: preparing a mask layer on the surface of the TCO layer of the solar cell precursor, and then etching the TCO layer outside the mask layer to form a grid line pattern; And / or, before the step of placing the solar cell precursor containing the grid line pattern in a copper mirror reaction solution for a reduction reaction, the method further includes: performing plasma treatment on the solar cell precursor containing the grid line pattern.

7. The preparation method according to claim 1, characterized in that: Before the step of removing the mask layer outside the gate line pattern and the copper seed layer on the mask layer, the method further includes: preparing a copper-nickel alloy plating layer on the surface of the copper plating layer by using an electroplating process; The thickness of the copper-nickel alloy plating layer is 2-5 μm; the mass ratio of copper to nickel in the copper-nickel alloy plating layer is (6-8) / (2-4).

8. The preparation method according to any one of claims 1 to 7, characterized in that: The thickness of the copper seed layer is 100-300 nm, and the thickness of the copper plating layer is 5-15 μm.

9. A low-cost solar cell electrode, characterized in that: A solar cell electrode prepared by the preparation method according to any one of claims 1 to 8.