Negative electrode material and preparation method thereof, negative electrode sheet and battery
Patent Information
- Application Number
- CN202411284336.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-13
AI Technical Summary
In existing secondary batteries, graphite, as the negative electrode material, has insufficient specific capacity, and it is difficult to meet the requirements of higher energy density. The volume of the selenide negative electrode material changes greatly during the charging and discharging process, resulting in a decrease in battery performance.
The negative electrode material with a core covered with zirconia and LiAlO2 layers is used to improve conductivity and structural stability through zirconia. LiAlO2 serves as a solid electrolyte interface mask to inhibit the side reaction of the electrolyte and the expansion of cobalt selenide.
It effectively reduces the DC internal resistance of the battery, improves stability and cycling performance, and improves the first Coulomb efficiency and cycling performance.
Smart Images

Figure CN118800913B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. Background Art
[0002] For secondary batteries, in order to obtain higher energy density, a negative electrode material with high specific capacity is needed to match it. Graphite, as a currently widely used negative electrode material, has an actual specific capacity below 372 mAh / g, which currently cannot meet the requirements for higher energy density of secondary batteries.
[0003] In recent years, selenide negative electrode materials have received extensive attention. Compared with traditional negative electrode materials, selenide materials have better plasticity and controllability in morphology, higher thermal stability and electrical conductivity, especially transition metal selenides, which have the advantages of high theoretical capacity and low potential, and have great potential for application in the field of electrochemistry.
[0004] However, during the battery charging and discharging reaction, the selenide negative electrode material will undergo serious volume changes, which can easily cause the electrode to pulverize, significantly reducing the battery performance. Summary of the invention
[0005] In view of this, the embodiments of the present application provide a negative electrode material and a preparation method thereof, a negative electrode plate and a battery to solve at least one problem existing in the background technology.
[0006] In a first aspect, an embodiment of the present application provides a negative electrode material, comprising a core and a first coating layer and a second coating layer sequentially coated on the surface of the core, wherein the material of the core comprises selenide, the material of the first coating layer comprises zirconium oxide, and the material of the second coating layer comprises LiAlO 2 .
[0007] In combination with the first aspect of the present application, in an optional embodiment, the material of the inner core includes at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide; and / or the particle size of the inner core is 9 μm~11 μm.
[0008] In combination with the first aspect of the present application, in an optional embodiment, the thickness of the first coating layer is 40nm~60nm; and / or the thickness of the second coating layer is 15nm~25nm.
[0009] In a second aspect, an embodiment of the present application provides a method for preparing a negative electrode material, the method comprising the following steps:
[0010] S1: dispersing selenide powder in a first solvent, adding zirconium oxide powder, and ball milling to form a zirconium oxide coating layer on the surface of the selenide powder to obtain a first coated selenide material;
[0011] S2: dispersing the first coated selenide material in an ammonium formate buffer solution, adding an aluminum source, stirring to carry out a chemical reaction, and forming an aluminum oxide coating layer on the surface of the first coated selenide material after centrifugation, washing and drying to obtain a second coated selenide material;
[0012] S3: The second coating selenide material is mixed evenly with lithium hydroxide monohydrate, and subjected to heat treatment, so that the aluminum oxide coating layer is formed into LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer is formed to obtain the negative electrode material.
[0013] In conjunction with the second aspect of the present application, in an optional implementation manner, step S1 satisfies at least one of the following features (1) to (6):
[0014] (1) The selenide powder includes at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide;
[0015] (2) the first solvent includes at least one of ethanol, ethylene glycol, benzyl alcohol, isopropanol, propanol, and methanol;
[0016] (3) The particle size of the zirconium oxide powder is 10 nm to 20 nm;
[0017] (4) The mass ratio of the selenide powder to the zirconium oxide powder is 1:(3-8);
[0018] (5) The rotation speed of the ball mill is 800 r / min~1100 r / min;
[0019] (6) The ball milling time is 0.5h~1.5h.
[0020] In conjunction with the second aspect of the present application, in an optional implementation manner, step S2 satisfies at least one of the following features (1) to (7):
[0021] (1) The molar concentration of the ammonium formate buffer solution is 0.2 mol / L-0.3 mol / L;
[0022] (2) The aluminum source includes at least one of aluminum sulfate, aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum acetate, and aluminum citrate;
[0023] (3) The mass ratio of the first coating selenide material to the aluminum source is 2:(3-7);
[0024] (4) The temperature of the chemical reaction is 65°C to 75°C;
[0025] (5) The chemical reaction time is 0.8h~1.1h;
[0026] (6) The drying temperature is 60°C to 80°C;
[0027] (7) The drying time is 4h~6h.
[0028] In conjunction with the second aspect of the present application, in an optional implementation manner, step S3 satisfies at least one of the following features (1) to (6):
[0029] (1) The mass ratio of the second coated selenide material to the lithium hydroxide monohydrate is 1:(3-5);
[0030] (2) The temperature of the heat treatment is 550°C to 750°C;
[0031] (3) The heat treatment holding time is 2.8h~3.2h;
[0032] (4) The heating rate of the heat treatment is 4.7°C / min to 5.3°C / min;
[0033] (5) LiAlO 2 The thickness of the coating layer is 15nm~25nm;
[0034] (6) The thickness of the zirconium oxide coating layer is 40nm~60nm.
[0035] In a third aspect, an embodiment of the present application provides a negative electrode plate, which includes the negative electrode material as described in the first aspect or includes the negative electrode material prepared by the preparation method as described in the second aspect.
[0036] In combination with the third aspect of the present application, in an optional embodiment, the negative electrode plate further includes a conductive agent and a binder, wherein the mass ratio of the negative electrode material, the conductive agent and the binder is (94~98): (0.5~1.5): (0.5~5.5).
[0037] In a fourth aspect, an embodiment of the present application provides a battery, comprising the negative electrode plate as described in the third aspect.
[0038] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0039] The negative electrode material and preparation method thereof, the negative electrode plate and the battery provided in the embodiment of the present application include a core and a first coating layer and a second coating layer sequentially coated on the surface of the core, wherein the material of the core includes selenide, the material of the first coating layer includes zirconium oxide, and the material of the second coating layer includes LiAlO 2 On the one hand, the first coating layer includes zirconium oxide with good conductivity, high thermal stability and high structural strength, which can improve the conductivity of the negative electrode material. Zirconium oxide can also strengthen the stability of the core lattice structure, inhibit the release of lattice oxygen, reduce the exothermic reaction between the negative electrode material and the electrolyte, and avoid local heat accumulation, thereby reducing the polarization and attenuation of the battery in a high temperature environment. Therefore, it can effectively reduce the DCR (Directive Current Resistance) of the battery and improve the stability, power performance and cycle performance of the battery. On the other hand, the second coating layer includes LiAlO 2 , LiAlO 2 It can be used as an artificial SEI (Solid Electrolyte Interface) membrane, which has uniform components, stable structure, and excellent electrochemical performance. It is conducive to the uniform diffusion of active ions, can effectively restrain the expansion of cobalt selenide in the core, and can prevent the electrolyte from reducing to form a SEI membrane on the surface of the negative electrode, reducing the side reactions of the electrolyte, thereby improving the first coulomb efficiency and cycle performance of the negative electrode material. In this way, by sequentially coating the first coating layer and the second coating layer on the surface of the core, the battery made of the negative electrode material can have a lower DCR and a higher first coulomb efficiency and cycle performance.
[0040] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0042] Figure 1 A schematic diagram of the structure of a negative electrode material provided in an embodiment of the present application;
[0043] Figure 2 A schematic diagram of a process for preparing a negative electrode material provided in an embodiment of the present application. DETAILED DESCRIPTION
[0044] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is described in detail by combining the accompanying drawings and listing specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional experimental conditions. The reagents and raw materials used in the present invention are commercially available unless otherwise specified.
[0045] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.
[0046] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0047] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.
[0048] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.
[0049] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values.
[0050] The present application embodiment provides a negative electrode material, such as Figure 1 As shown, the negative electrode material includes a core 100 and a first coating layer 101 and a second coating layer 102 sequentially coated on the surface of the core, wherein the material of the core 100 includes selenide, the material of the first coating layer 101 includes zirconium oxide, and the material of the second coating layer 102 includes LiAlO 2.
[0051] In the embodiment of the present application, on the one hand, the first coating layer 101 includes zirconium oxide with good conductivity, high thermal stability and high structural strength, which can improve the conductivity of the negative electrode material. Zirconium oxide can also strengthen the stability of the core lattice structure, inhibit the release of lattice oxygen, reduce the exothermic reaction between the negative electrode material and the electrolyte, and avoid local heat accumulation, thereby reducing the polarization and attenuation of the battery in a high temperature environment. Therefore, the DCR of the battery can be effectively reduced, and the stability, power performance and cycle performance of the battery can be improved. On the other hand, the second coating layer 102 includes LiAlO 2 , LiAlO 2 As a solid electrolyte, LiAlO has good ionic conductivity and poor electronic conductivity, which can effectively inhibit the contact between the electrolyte and the electrode material surface and the electron transfer. 2 It can be used as an artificial SEI membrane, which has uniform components, stable structure, and excellent electrochemical performance, is conducive to the uniform diffusion of active ions, can effectively restrain the expansion of cobalt selenide in the core 100, and can prevent the electrolyte from reducing to form an SEI membrane on the surface of the negative electrode, which is equivalent to forming an SEI membrane in the battery system in advance, reducing the side reactions of the electrolyte, thereby improving the first coulomb efficiency and cycle performance of the negative electrode material. Moreover, the artificial SEI membrane can be designed according to actual needs, so that it has a better morphology structure and structural strength, and can more effectively restrain the expansion of the cobalt selenide negative electrode material. In this way, by sequentially coating the first coating layer 101 and the second coating layer 102 on the surface of the core 100, the battery made of the negative electrode material can have a lower DCR and a higher first coulomb efficiency and cycle performance.
[0052] It should be noted that the first coating layer 101 in the embodiment of the present application substantially covers the entire surface of the core 100. Here, “substantially” can be understood as, within the tolerance of the process in the art, the first coating layer 101 covers the entire surface of the core 100. Similarly, the second coating layer 102 in the embodiment of the present application substantially covers the entire surface of the first coating layer 101. It can be considered that, within the tolerance of the process in the art, the second coating layer 102 covers the entire surface of the first coating layer 101.
[0053] In the embodiment of the present application, the material of the core 100 may include, for example, a transition metal selenide, because the transition metal selenide has a higher theoretical capacity and a lower potential, and can effectively improve the capacity performance and electrochemical performance of the negative electrode material. In some specific embodiments, the material of the core 100 may include, for example, at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide.
[0054] In some embodiments, the particle size of the core 100 may be 9 μm to 11 μm, for example, 9 μm, 10 μm, 11 μm, or any value between any two of the above ranges. The particle size of the core 100 is within the above range, so that the particle size of the negative electrode material is within a suitable range, so that the negative electrode material can exert better electrochemical performance.
[0055] In the embodiment of the present application, when the thickness of the first coating layer 101 is small, the structural strength of the first coating layer 101 is relatively weak, and the effect of reducing DCR and improving battery stability and power performance is not obvious enough. When the thickness of the first coating layer 101 is large, the transmission path of the active ions will be extended, affecting the migration of the active ions in the negative electrode material. Therefore, in some specific embodiments, the thickness of the first coating layer 101 can be 40nm~60nm, for example, 40nm, 45nm, 50nm, 55nm, 60nm or any value between any two of the above numerical ranges.
[0056] In the embodiment of the present application, when the thickness of the second coating layer 102 is small, the structural strength of the second coating layer 102 is relatively weak, and the effect on the expansion of bound cobalt selenide and the effect on improving the first coulombic efficiency and cycle performance is relatively limited. When the thickness of the second coating layer 102 is large, the transmission path of the active ions will be extended, affecting the migration of the active ions in the negative electrode material. Therefore, in some specific embodiments, the thickness of the second coating layer 102 can be 15nm~25nm, for example, it can be 15nm, 20nm, 25nm or any value between any two of the above numerical ranges.
[0057] The present application also provides a method for preparing a negative electrode material. Figure 2 The method for preparing the negative electrode material provided in the embodiment of the present application comprises the following steps:
[0058] S1: dispersing selenide powder in a first solvent, adding zirconium oxide powder, and ball milling to form a zirconium oxide coating layer on the surface of the selenide powder to obtain a first coated selenide material;
[0059] S2: dispersing the first coated selenide material in an ammonium formate buffer solution, adding an aluminum source, stirring to carry out a chemical reaction, and forming an aluminum oxide coating layer on the surface of the first coated selenide material after centrifugation, washing and drying to obtain a second coated selenide material;
[0060] S3: The second coating selenide material is mixed evenly with lithium hydroxide monohydrate, and heat treated so that the aluminum oxide coating layer is formed into LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer is formed to obtain the negative electrode material.
[0061] In the embodiment of the present application, on the one hand, a zirconium oxide coating layer is formed on the surface of the selenide. Since zirconium oxide has good conductivity, high thermal stability and high structural strength, it can improve the conductivity of the negative electrode material. Zirconium oxide can also strengthen the stability of the core lattice structure, inhibit the release of lattice oxygen, reduce the exothermic reaction between the negative electrode material and the electrolyte, avoid local heat accumulation, and thus reduce the polarization and attenuation of the battery in a high temperature environment. Therefore, it can effectively reduce the DCR of the battery and improve the stability, power performance and cycle performance of the battery. On the other hand, LiAlO is formed on the surface of the zirconium oxide coating layer. 2 Coating layer, LiAlO 2 As a solid electrolyte, LiAlO has good ionic conductivity and poor electronic conductivity, which can effectively inhibit the contact between the electrolyte and the electrode material surface and the electron transfer. 2 It can be used as an artificial SEI membrane, which has uniform components, stable structure, and excellent electrochemical performance. It is conducive to the uniform diffusion of active ions, can effectively restrain the expansion of cobalt selenide, and can prevent the electrolyte from reducing to form an SEI membrane on the negative electrode surface, which is equivalent to forming an SEI membrane in the battery system in advance, reducing the side reactions of the electrolyte, thereby improving the first coulombic efficiency and cycle performance of the negative electrode material. Moreover, the artificial SEI membrane can be designed according to actual needs, so that it has a better morphology structure and structural strength, and can more effectively restrain the expansion of cobalt selenide negative electrode materials. In this way, by sequentially forming a zirconium oxide coating layer and a LiAlO 2 The coating layer can make the battery made of the negative electrode material have a lower DCR and a higher first coulombic efficiency and cycle performance.
[0062] In some embodiments, the selenide powder may include at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide.
[0063] There is no particular limitation on the type of the first solvent in step S1, and it can be selected according to actual needs. For example, the first solvent can include at least one of ethanol, ethylene glycol, benzyl alcohol, isopropanol, propanol, and methanol.
[0064] The particle size of the zirconium oxide powder in step S1 can be 10nm~20nm, for example, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm or any value between any two of the above numerical ranges. Nano-scale zirconium oxide powder can form a dense and high-quality zirconium oxide coating layer on the surface of the selenide powder. Controlling the particle size of the zirconium oxide powder within the above range is conducive to forming a denser and higher-quality zirconium oxide coating layer, thereby better improving the stability and electrochemical performance of the negative electrode material.
[0065] When the mass ratio of the selenide powder to the zirconium oxide powder is relatively large, the integrity and quality of the zirconium oxide coating formed on the surface of the selenide powder will be affected. When the mass ratio of the selenide powder to the zirconium oxide powder is relatively small, the zirconium oxide powder will form agglomerations, thereby increasing the surface area, introducing defects, and the thickness of the formed zirconium oxide coating is relatively large, which will affect the migration of active ions in the negative electrode material. Therefore, in some specific embodiments, the mass ratio of the selenide powder to the zirconium oxide powder can be 1: (3-8), for example, it can be 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8 or any value between any two of the above numerical ranges, so as to facilitate the formation of a complete, high-quality zirconium oxide coating with appropriate thickness, thereby further improving the stability and electrochemical performance of the negative electrode material.
[0066] The ball milling step in step S1 may specifically be: firstly disperse the selenide powder in the first solvent, add the zirconium oxide powder, and then use a planetary ball mill for ball milling, and the ball milling speed may be 800r / min~1100r / min, for example, 800r / min, 900r / min, 1000r / min, 1100r / min or any value between any two of the above numerical ranges. Controlling the ball milling speed within the above range is conducive to forming a more uniform and complete zirconium oxide coating layer, avoiding damage to the material structure, and controlling the particle size of the material after ball milling within a suitable range, so as to facilitate the final preparation of a negative electrode material with higher quality.
[0067] In some specific embodiments, the ball milling time can be 0.5h~1.5h, for example, it can be 0.5h, 0.75h, 1h, 1.25h, 1.5h or any value between any two of the above numerical ranges. This can further improve the uniformity and integrity of the zirconia coating layer, and form a material with suitable and uniform particle size, so as to ultimately obtain a higher quality negative electrode material.
[0068] The molar concentration of the ammonium formate buffer solution in step S2 can be 0.2mol / L-0.3mol / L, for example, it can be 0.2mol / L, 0.25mol / L, 0.3mol / L or any value between any two of the above numerical ranges. By controlling the molar concentration of the ammonium formate buffer solution within the above range, the reaction system can be controlled in a more stable state, which is beneficial to promoting the aluminum oxide reaction, thereby forming a better aluminum oxide coating layer.
[0069] There is no particular limitation on the type of aluminum source in step S2, and it can be selected according to actual needs.
[0070] The aluminum source refers to a compound for providing aluminum. For example, the aluminum source may include at least one of aluminum sulfate, aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum acetate, and aluminum citrate.
[0071] When the mass ratio of the first coating selenide material to the aluminum source is relatively large, the content of the aluminum source is relatively small, and the content of the reactants is low, which is not conducive to full reaction. The integrity and quality of the aluminum oxide coating layer formed on the surface of the first coating selenide material will be affected. When the mass ratio of the first coating selenide material to the aluminum source is relatively small, the content of the aluminum source is relatively high, which will affect the crystal nucleation of the coating layer, resulting in crystal defects, thereby affecting the coating effect. Therefore, in some specific embodiments, the mass ratio of the first coating selenide material to the aluminum source can be 2: (3~7), for example, it can be 2: 3, 2: 4, 2: 5, 2: 6, 2: 7 or any value between any two of the above numerical ranges, so as to facilitate the formation of a complete, high-quality aluminum oxide coating layer with appropriate thickness, thereby facilitating the formation of high-quality LiAlO in the next step. 2 Coating layer.
[0072] The temperature of the chemical reaction in step S2 is closely related to the quality of the formed aluminum oxide coating layer. Therefore, in some embodiments, the temperature of the chemical reaction can be 65°C to 75°C, for example, 65°C, 70°C, 75°C or any value between any two of the above ranges. Controlling the reaction temperature within the above range can promote the chemical reaction, thereby forming an aluminum oxide coating layer with better quality.
[0073] In actual operation, after the first coated selenide material is dispersed in the ammonium formate buffer solution, it can be heated and kept at 65°C to 75°C in a water bath or an oil bath, and then the aluminum source is added and stirred vigorously to react. In some specific embodiments, an oil bath can be used for heating and keeping warm, because the oil bath has a higher heat transfer efficiency and a faster heating speed.
[0074] The time of the chemical reaction in step S2 is closely related to the quality of the formed aluminum oxide coating layer. Therefore, in some embodiments, the time of the chemical reaction can be 0.8h~1.1h, for example, 0.8h, 0.9h, 1h, 1.1h or any value between any two of the above numerical ranges. Controlling the time of the chemical reaction within the above range can make the chemical reaction proceed more fully, thereby forming an aluminum oxide coating layer with better quality.
[0075] In step S2, after the chemical reaction is completed, centrifugation, washing and drying are performed in sequence, wherein the centrifugation can adopt a centrifugation process well known to those skilled in the art, which will not be described in detail here. Washing can be performed using ethanol and water respectively, for example, first washing with ethanol 2 to 3 times, and then washing with water 2 to 3 times to fully remove the residual reactants. The drying temperature can be 60°C to 80°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C or any value between any two of the above numerical ranges, so that the moisture can be removed quickly while avoiding affecting the material itself.
[0076] Furthermore, the drying time can be 4h~6h, for example, 4h, 4.5h, 5h, 5.5h, 6h or any value between any two of the above numerical ranges, so that the moisture in the material can be fully removed to obtain a second coated selenide material with better quality.
[0077] The specific operation in step S3 can be firstly mixing the second coated selenide material and lithium hydroxide monohydrate evenly in a mortar, and then placing them in a tube furnace for heat treatment.
[0078] When the mass ratio of the second coating selenide material to lithium hydroxide monohydrate is relatively large, it is not conducive to fully forming the aluminum oxide coating layer into LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer will affect the stability and electrochemical performance of the prepared negative electrode material. When the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is small, the content of lithium hydroxide monohydrate is relatively too high. Too high an addition amount will cause the coating material to agglomerate, thereby increasing the surface area of the negative electrode material, resulting in increased consumption of the electrolyte, causing the DC internal resistance of the battery to grow faster, thereby deteriorating the power performance. Therefore, in some specific embodiments, the mass ratio of the second coated selenide material to lithium hydroxide monohydrate can be 1: (3-5), for example, 1: 3, 1: 4, 1: 5 or any value between any two of the above numerical ranges, which is conducive to obtaining a negative electrode material with higher quality.
[0079] Heat treatment temperature and LiAlO 2 The formation of the coating layer is closely related to the quality of the final negative electrode material.
[0080] In some embodiments, the heat treatment temperature may be 550°C to 750°C, for example, 550°C, 600°C, 650°C, 700°C, 750°C or any value between any two of the above ranges, which can further promote the aluminum oxide coating layer in the second coating selenide material to better form LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer further improves the quality of the obtained negative electrode material.
[0081] In some embodiments, the heat treatment holding time can be 2.8 h to 3.2 h, for example, 2.8 h, 2.9 h, 3 h, 3.1 h, 3.2 h or any value between any two of the above ranges, which is conducive to forming a more uniform and higher quality LiAlO 2 The coating layer further improves the quality of the obtained negative electrode material.
[0082] In some embodiments, the heating rate of the heat treatment can be 4.7°C / min to 5.3°C / min, for example, 4.7°C / min, 4.8°C / min, 4.9°C / min, 5°C / min, 5.1°C / min, 5.2°C / min, 5.3°C / min or any value between any two of the above numerical ranges, so that the material can be heated more evenly during the heat treatment heating process, that is, the temperature distribution inside the material is relatively uniform, which is conducive to better forming the LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer further improves the quality of the obtained negative electrode material.
[0083] In some embodiments, the thickness of the zirconium oxide coating layer in the prepared negative electrode material can be 40nm~60nm, for example, 40nm, 45nm, 50nm, 55nm, 60nm or any value between any two of the above numerical ranges, so that the stability of the zirconium oxide coating layer can be better, and the effect of reducing DCR and improving the stability and power performance of the battery can be better.
[0084] In some embodiments, the LiAlO in the prepared negative electrode material 2 The thickness of the coating layer can be 15 nm to 25 nm, for example, 15 nm, 20 nm, 25 nm or any value between any two of the above numerical ranges, which can further improve the first coulombic efficiency and cycle performance of the negative electrode material.
[0085] Based on this, an embodiment of the present application further provides a negative electrode plate, comprising the negative electrode material described in any of the above embodiments or the negative electrode material prepared by the preparation method described in any of the above embodiments.
[0086] It should be understood that since the negative electrode plate in the embodiments of the present application includes the negative electrode material described in any of the above embodiments or includes the negative electrode material prepared by the preparation method described in any of the above embodiments, the beneficial effects of the negative electrode material described in any of the above embodiments are applicable to the negative electrode plate.
[0087] In some embodiments, the negative electrode plate may further include a conductive agent and a binder, wherein the mass ratio of the negative electrode material, the conductive agent and the binder may be (94-98): (0.5-1.5): (0.5-5.5). By controlling the mass ratio of the negative electrode material, the conductive agent and the binder, a negative electrode plate with higher performance may be obtained.
[0088] Exemplarily, the conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, and conductive graphite; the binder may include at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyacrylates, and polyacrylic acid.
[0089] In some embodiments, the negative electrode plate may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer may include the negative electrode material described in any of the aforementioned embodiments.
[0090] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode active material layer is disposed on either or both of the two facing surfaces of the negative electrode current collector.
[0091] The present application has no particular restrictions on the preparation method of the negative electrode sheet, and any preparation method known in the art may be selected as long as the purpose of the present application can be achieved.
[0092] Based on this, an embodiment of the present application also provides a battery, comprising the negative electrode plate described in the above embodiment.
[0093] It should be understood that, since the battery in the embodiment of the present application includes the negative electrode plate described in the above embodiment, the beneficial effects of the negative electrode plate described in any of the above embodiments are applicable to the battery.
[0094] In some embodiments, the battery may be a secondary battery, and the secondary battery may be a lithium-ion secondary battery. Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0095] The technical solution of the present application is further described below in combination with a plurality of embodiments and comparative examples. Example 1
[0096] The preparation of the negative electrode material in this embodiment includes the following steps:
[0097] S101: firstly, dispersing CoSe powder in anhydrous ethanol, adding nano zirconium oxide powder to obtain a mixed material, wherein the mass ratio of CoSe powder to zirconium oxide powder is 1:5, and then placing the mixed material in a planetary ball mill for ball milling, the ball mill speed is 900 r / min, the ball milling time is 1 h, and obtaining a zirconium oxide-coated cobalt selenide modified material (first coated selenide material);
[0098] S201: firstly, the first coated selenide material obtained in step S101 is dispersed in 300 mL of 0.2 mol / L ammonium formate buffer solution, heated in an oil bath and kept at 70°C, then aluminum sulfate is added, and the chemical reaction is carried out with vigorous stirring for 1 hour, wherein the mass ratio of the first coated selenide material to aluminum sulfate is 2:5, and then the solution is centrifuged and washed twice with ethanol and then with water, and then dried at 70°C for 6 hours to obtain a cobalt selenide modified material (second coated selenide material) in which the second coating layer is aluminum oxide and the first coating layer is zirconium oxide;
[0099] S301: First, the second coated selenide material obtained in step S201 is evenly mixed with lithium hydroxide monohydrate in a mortar, wherein the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is 1:4, and then placed in a tubular furnace for high-temperature annealing treatment (heat treatment), the heating rate of the heat treatment is 5°C / min, the heat treatment temperature is 650°C, and the heat treatment holding time is 3h. After the heat treatment is completed, the negative electrode material is obtained. Example 2
[0100] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the mass ratio of CoSe powder to zirconium oxide powder in step S101 is 1:3. Example 3
[0101] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the mass ratio of CoSe powder to zirconium oxide powder in step S101 is 1:8. Example 4
[0102] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the rotation speed of the ball mill in step S101 is 800 r / min. Example 5
[0103] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the rotation speed of the ball mill in step S101 is 1100 r / min. Example 6
[0104] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that in step S201, the mass ratio of the first coating selenide material to aluminum sulfate is 2:3. Example 7
[0105] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that in step S201, the mass ratio of the first coating selenide material to aluminum sulfate is 2:7. Example 8
[0106] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that: in step S201, the chemical reaction is carried out by vigorous stirring for 0.8 h. Example 9
[0107] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that: in step S201, the chemical reaction is carried out by vigorous stirring for 1.1 h. Example 10
[0108] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that in step S301, the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is 1:3. Embodiment 11
[0109] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that in step S301, the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is 1:5. Example 12
[0110] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the temperature of the heat treatment in step S301 is 550°C. Embodiment 13
[0111] The preparation of the negative electrode material in this embodiment is basically the same as that in Embodiment 1, except that the temperature of the heat treatment in step S301 is 750° C. Comparative Example 1
[0112] The preparation of the negative electrode material in this comparative example is basically the same as that in Example 1, except that no nano zirconium oxide powder is added in step S101. Comparative Example 2
[0113] The preparation of the negative electrode material in this comparative example is basically the same as that in Example 1, except that: lithium hydroxide monohydrate is not added in step S301.
[0114] The negative electrode materials obtained in the above-mentioned embodiments and comparative examples were made into lithium-ion batteries, and the performance of the batteries was tested.
[0115] The preparation of lithium-ion batteries includes the following steps:
[0116] Preparation of positive electrode sheets: first, lithium iron phosphate, conductive agent acetylene black, and binder PVDF are mixed in a mass ratio of 97:1:2, solvent N-methylpyrrolidone is added, and the mixture is stirred under the action of a vacuum mixer until the system becomes uniform to obtain positive electrode slurry; then, the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain positive electrode sheets.
[0117] Preparation of negative electrode sheets: first, the negative electrode materials obtained in the above embodiments and comparative examples, conductive carbon black (super-P), sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.4:1:1.2:1.4, and deionized water is added as a solvent. The mixture is stirred under the action of a vacuum mixer until the system becomes uniform to obtain a negative electrode slurry; then, the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain a negative electrode sheet.
[0118] Prepare the electrolyte: Mix ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1, and then add 1 mol / L LiPF 6 Mix well to prepare electrolyte.
[0119] Preparation of batteries: The positive electrode sheet, separator and negative electrode sheet are stacked in sequence, then wound into a battery cell and loaded into an aluminum shell. After processes such as liquid injection, formation and capacity division, a lithium-ion battery is obtained.
[0120] Performance testing of lithium-ion batteries, including:
[0121] (1) First coulombic efficiency (first efficiency) test:
[0122] 0.1C charging capacity: 0.1C constant current and constant voltage charging to 3.65V, the cut-off current is 0.05C, and it is left to stand for 5 minutes. The capacity measured in this step is the 0.1C charging capacity (recorded as C0).
[0123] 0.1C discharge capacity: Discharge at 0.1C constant current to 2.5V and let stand for 5 minutes. The capacity measured in this step is the 0.1C discharge capacity (denoted as C1).
[0124] The first effect is: C1 / C0.
[0125] (2) Cyclic performance test:
[0126] Charging: 1C constant current and constant voltage charging to 3.65V, cut-off current is 0.05C, and stand for 5 minutes; Discharging: 1C constant current discharge to 2.5V, stand for 5 minutes. Completing one charging and discharging process is considered to complete one cycle.
[0127] Discharge capacity after the first cycle of 1C operation: 1C constant current and constant voltage charging to 3.65V, the cut-off current is 0.05C, and 1C constant current discharge to 2.5V. The discharge capacity measured in this step is the discharge capacity of the first cycle of 1C operation (recorded as C3).
[0128] Discharge capacity when 1C runs to the 2500th cycle: 1C constant current and constant voltage charging to 3.65V, the cut-off current is 0.05C, and 1C constant current discharge to 2.5V. The discharge capacity measured in this step is the discharge capacity when 1C runs to 2500 cycles (recorded as C4).
[0129] The capacity retention rate after running 2500 cycles at 1C is: C4 / C3.
[0130] (3) DCR test: 1C constant current and constant voltage charging to 50% SOC (State of Charge), capacity cutoff, voltage recorded as U0, 2C constant current discharge for 30s, voltage recorded as U1, DCR = (U0-U1) / I, I = 2C1.
[0131] The test results of the battery performance are shown in Table 1.
[0132] Table 1
[0133]
[0134] From the data in Table 1, it can be seen that the battery prepared by using the negative electrode materials prepared in Examples 1 to 13 not only has a low DCR, but also has a high initial efficiency and a long cycle life. It can be seen that the negative electrode material in the present application comprises a selenide and a zirconium oxide coating layer and a LiAlO coating layer sequentially coated on the surface of the selenide. 2 The coating layer makes the battery made of negative electrode materials have lower DCR and higher first coulomb efficiency and cycle performance. This is because zirconium oxide has good conductivity, high thermal stability and high structural strength, which can improve the conductivity of negative electrode materials. Elemental zirconium can inhibit the release of lattice oxygen, reduce the exothermic reaction between electrode materials and electrolytes, thereby avoiding local heat accumulation, inhibiting the structural degradation of negative electrode materials at high temperatures and the generation of gas, thereby reducing the polarization and attenuation of the battery in a high temperature environment, thereby improving the stability of the battery and high-temperature cycle performance. At the same time, because the nano zirconium oxide lattice is larger, it can effectively improve the diffusion capacity of active ions, such as lithium ions, thereby effectively reducing DCR and improving the power performance of the battery. In addition, LiAlO 2 As a solid electrolyte, LiAlO has good ionic conductivity and poor electronic conductivity, which can effectively inhibit the contact between the electrolyte and the electrode material surface and the electron transfer. 2It can be used as an artificial SEI membrane with uniform components, stable structure, and excellent electrochemical performance. It is conducive to the uniform diffusion of active ions, can effectively restrain the expansion of cobalt selenide, and can prevent the electrolyte from being reduced to form a SEI membrane on the negative electrode surface, which is equivalent to forming a SEI membrane in the battery system in advance, reducing the side reactions of the electrolyte, thereby improving the first coulombic efficiency and cycle performance of the negative electrode material.
[0135] From the results of Examples 1 to 3 in Table 1, it can be seen that the performance of the obtained negative electrode material is better when the mass ratio of cobalt selenide powder to zirconium oxide powder is controlled within an appropriate range. Therefore, the battery prepared using the obtained negative electrode material has a smaller DCR, a longer cycle life, and a higher first efficiency. This is because when the mass ratio of cobalt selenide powder to zirconium oxide powder is relatively large, that is, when the content of zirconium oxide powder is low, a relatively complete coating cannot be formed. When the mass ratio of cobalt selenide powder to zirconium oxide powder is relatively small, that is, when the content of zirconium oxide powder is high, the zirconium oxide powder will form agglomerates, thereby increasing the surface area, introducing defects, and affecting the quality of the negative electrode material. Therefore, it is more appropriate that the mass ratio of cobalt selenide powder to zirconium oxide powder is in the range of 1: (3~8).
[0136] From the results of Example 1, Example 4 and Example 5 in Table 1, it can be seen that the performance of the obtained negative electrode material is better when the ball milling speed is controlled within a suitable range. Therefore, the battery prepared using the obtained negative electrode material has a smaller DCR, a longer cycle life and a higher first efficiency. This is because when the ball milling speed is low, the coating material zirconium oxide powder cannot be evenly dispersed, which is not conducive to forming a uniform, high-quality zirconium oxide coating layer. When the ball milling speed is high, it is easy to cause material structure damage, and the battery performance prepared by the obtained negative electrode material will be reduced. Therefore, the ball milling speed is more suitable in the range of 800r / min~1100r / min.
[0137] From the results of Example 1, Example 6 and Example 7 in Table 1, it can be seen that the mass ratio of the first coated selenide material to aluminum sulfate is controlled within a suitable range, and the performance of the obtained negative electrode material is better. Therefore, the battery prepared using the obtained negative electrode material has a smaller DCR, a longer cycle life, and a higher first efficiency. When the mass ratio of the first coated selenide material to aluminum sulfate is relatively large, the content of aluminum sulfate is relatively small, and the content of reactants is low, which is not conducive to sufficient reaction to form a good aluminum oxide coating layer. When the mass ratio of the first coated selenide material to aluminum sulfate is small, the content of aluminum sulfate is relatively high, which will affect the nucleation of the coating layer crystals, resulting in crystal defects, thereby affecting the coating effect. Therefore, it is more appropriate that the mass ratio of the first coated selenide material to the aluminum source is in the range of 2: (3~7).
[0138] From the results of Example 1, Example 8 and Example 9 in Table 1, it can be seen that the chemical reaction time of the first coated selenide material and aluminum sulfate is controlled within a suitable range, and the performance of the obtained negative electrode material is better. Therefore, the DCR of the battery prepared by using the obtained negative electrode material is small, the cycle life is long, and the first efficiency is high. Because when the chemical reaction time is short, the coating layer formed is thinner, the structural strength is weak, and it is impossible to fully cope with the destruction and reconstruction of the SEI film during the cycle, which will affect the high temperature cycle performance of the battery. When the chemical reaction time is long, the coating layer formed is thicker, which will affect the migration of active ions in the negative electrode material, thereby weakening the power performance of the negative electrode material. Therefore, it is more appropriate for the chemical reaction time to be in the range of 0.8h~1.1h.
[0139] From the results of Example 1, Example 10 and Example 11 in Table 1, it can be seen that when the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is controlled within an appropriate range, the performance of the obtained negative electrode material is better. Therefore, the battery prepared using the obtained negative electrode material has a smaller DCR, a longer cycle life and a higher initial efficiency. This is because when the mass ratio of the second coated selenide material to lithium hydroxide monohydrate is large, that is, when the content of lithium hydroxide monohydrate is too low, the alumina coating layer cannot be completely converted into LiAlO 2 The coating layer will lead to coating defects, which is not conducive to the battery cycle performance and the first effect. When the mass ratio of the second coating selenide material to lithium hydroxide monohydrate is small, that is, when the content of lithium hydroxide monohydrate is too high, the excessive addition will lead to the agglomeration of the coating material, thereby increasing the surface area of the negative electrode material, resulting in increased consumption of the electrolyte, and making the DC internal resistance of the battery grow faster, thereby deteriorating the power performance. Therefore, the mass ratio of the second coating selenide material to lithium hydroxide monohydrate is more suitable in the range of 1: (3~5).
[0140] From the results of Example 1, Example 12 and Example 13 in Table 1, it can be seen that the temperature of the heat treatment of the second coated selenide material and the monohydrated lithium hydroxide is controlled within a suitable range, and the performance of the obtained negative electrode material is better. Therefore, the DCR of the battery prepared by using the obtained negative electrode material is small, the cycle life is long, and the first efficiency is high. Because when the temperature of the heat treatment is too low, the material crystallinity is small, which is not conducive to the formation of a complete lattice and grains, and the material defects are more. When the temperature of the heat treatment is too high, the particles will grow to form larger grains, which is not conducive to reducing the decomposition potential, thereby causing the power and cycle and storage performance of the lithium-ion battery to decrease. Therefore, it is more appropriate to control the temperature of the heat treatment within the range of 550°C to 750°C.
[0141] From the results of Example 1 and Comparative Example 1 in Table 1, it can be seen that in Comparative Example 1, since nano zirconium oxide powder is not added in step S101, a nano zirconium oxide coating layer cannot be formed on the surface of the selenide powder, and the DCR of the battery prepared by the obtained negative electrode material is greatly increased, which will seriously affect the power performance of the battery and result in low overall performance of the battery.
[0142] From the results of Example 1 and Comparative Example 2 in Table 1, it can be seen that in Comparative Example 2, no lithium hydroxide monohydrate was added in step S301, resulting in failure to form LiAlO 2 The first efficiency and high-temperature cycle performance of the battery prepared with the negative electrode material obtained by the artificial SEI film are greatly reduced and cannot meet the design requirements.
[0143] It should be noted that the negative electrode material embodiments, negative electrode material preparation method embodiments, negative electrode plate embodiments and battery embodiments provided in the present application belong to the same concept; the technical features in the technical solutions recorded in each embodiment can be arbitrarily combined without conflict.
[0144] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.
Claims
1. A negative electrode material, It is characterized in that The invention comprises a core and a first coating layer and a second coating layer sequentially coated on the surface of the core, wherein the material of the core comprises selenide, the material of the first coating layer comprises zirconium oxide, and the material of the second coating layer comprises LiAlO 2 .
2. The negative electrode material according to claim 1, It is characterized in that The material of the core includes at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide; and / or, The particle size of the core is 9 μm to 11 μm.
3. The negative electrode material according to claim 1 or 2, It is characterized in that The thickness of the first coating layer is 40nm~60nm; and / or, The thickness of the second coating layer is 15nm~25nm.
4. A method for preparing a negative electrode material, It is characterized in that The method comprises the following steps: S1: dispersing selenide powder in a first solvent, adding zirconium oxide powder, and ball milling to form a zirconium oxide coating layer on the surface of the selenide powder to obtain a first coated selenide material; S2: dispersing the first coated selenide material in an ammonium formate buffer solution, adding an aluminum source, stirring to carry out a chemical reaction, and forming an aluminum oxide coating layer on the surface of the first coated selenide material after centrifugation, washing and drying to obtain a second coated selenide material; S3: The second coating selenide material is mixed evenly with lithium hydroxide monohydrate, and subjected to heat treatment, so that the aluminum oxide coating layer is formed into LiAlO coated on the surface of the zirconium oxide coating layer. 2 The coating layer is formed to obtain the negative electrode material.
5. The method for preparing the negative electrode material according to claim 4, It is characterized in that Step S1 satisfies at least one of the following characteristics (1) to (6): (1) The selenide powder includes at least one of cobalt selenide, cobalt diselenide, nickel selenide, nickel diselenide, manganese selenide, ferrous selenide, ferrous diselenide, and iron tetraselenide; (2) the first solvent includes at least one of ethanol, ethylene glycol, benzyl alcohol, isopropanol, propanol, and methanol; (3) The particle size of the zirconium oxide powder is 10 nm to 20 nm; (4) The mass ratio of the selenide powder to the zirconium oxide powder is 1:(3-8); (5) The rotation speed of the ball mill is 800 r / min~1100 r / min; (6) The ball milling time is 0.5h~1.5h.
6. The method for preparing the negative electrode material according to claim 4, It is characterized in that Step S2 satisfies at least one of the following characteristics (1) to (7): (1) The molar concentration of the ammonium formate buffer solution is 0.2 mol / L-0.3 mol / L; (2) The aluminum source includes at least one of aluminum sulfate, aluminum chloride hexahydrate, aluminum nitrate nonahydrate, aluminum acetate, and aluminum citrate; (3) The mass ratio of the first coating selenide material to the aluminum source is 2:(3-7); (4) The temperature of the chemical reaction is 65°C to 75°C; (5) The chemical reaction time is 0.8h~1.1h; (6) The drying temperature is 60°C to 80°C; (7) The drying time is 4h~6h.
7. The method for preparing the negative electrode material according to claim 4, It is characterized in that Step S3 satisfies at least one of the following characteristics (1) to (6): (1) The mass ratio of the second coated selenide material to the lithium hydroxide monohydrate is 1:(3-5); (2) The temperature of the heat treatment is 550°C to 750°C; (3) The heat treatment holding time is 2.8h~3.2h; (4) The heating rate of the heat treatment is 4.7°C / min to 5.3°C / min; (5) LiAlO 2 The thickness of the coating layer is 15nm~25nm; (6) The thickness of the zirconium oxide coating layer is 40nm~60nm.
8. A negative electrode sheet, It is characterized in that The invention comprises the negative electrode material according to any one of claims 1 to 3 or the negative electrode material prepared by the preparation method according to any one of claims 4 to 7.
9. The negative electrode sheet according to claim 8, It is characterized in that The negative electrode plate also includes a conductive agent and a binder, wherein the mass ratio of the negative electrode material, the conductive agent and the binder is (94-98): (0.5-1.5): (0.5-5.5).
10. A battery, It is characterized in that Comprising the negative electrode sheet as described in claim 8 or 9.