Preparation method of anti-fouling and acid-resistant nanofiltration membrane applied to high-salinity water

By using sulfonated two-dimensional porous materials with dopamine and piperazine on the nanofiltration membrane to construct an active separation layer, the problems of poor fouling resistance and easy acid decomposition of traditional nanofiltration membranes in high salt water are solved, and the permeation flux is achieved. and improved separation selectivity, demonstrating excellent antifouling and acid resistance properties.

CN118807463APending Publication Date: 2024-10-22TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410994595.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Traditional nanofiltration membranes have problems such as poor anti-fouling properties, easy acid hydrolysis, reduced permeability flux, and reduced separation selectivity in high salt water separation, which limits their application scope.

Method used

Sulfonated two-dimensional porous materials (COFs-SO3H) are used with dopamine and piperazine to construct an active separation layer through interfacial polymerization to form a nanofiltration membrane with an acid-resistant skeleton structure and hydrophilic functional groups to regulate the surface charge properties of the functional layer. and micro-nano structure to improve anti-fouling and acid resistance.

Benefits of technology

It achieves simultaneous improvement in permeability flux and water-salt separation selectivity in high salt water, and exhibits excellent anti-fouling and acid resistance properties, expanding the application potential of nanofiltration membranes in the field of high-salt solution separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807463A_ABST
    Figure CN118807463A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of membrane material preparation and membrane separation, and relates to a preparation method of an anti-fouling and acid-resistant nanofiltration membrane applied to high-salinity water, which comprises the following steps: taking an ultrafiltration basement membrane as a substrate, and infiltrating the basement membrane by using a prepared aqueous phase solution under the assistance of pressure to obtain the ultrafiltration basement membrane with an aqueous phase functional layer; and pouring the oil phase solution into an ultrafiltration basement membrane, carrying out interfacial polymerization reaction, washing the surface with an n-hexane solution, and carrying out heat treatment in a drying oven to obtain the anti-fouling and acid-resistant nanofiltration membrane. The prepared nanofiltration membrane shows synchronous improvement of permeation flux and water-salt separation selectivity in a strong brine separation process, and shows excellent anti-pollution and acid-resistant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane material preparation and membrane separation, and in particular relates to a method for preparing a fouling-resistant and acid-resistant nanofiltration membrane used in high-salt water. Background Art

[0002] Concentrated brine, especially the comprehensive utilization and zero discharge of concentrated brine after seawater desalination, has received extensive attention. High concentration of sodium chloride in concentrated seawater is an important basic raw material for the chlor-alkali industry. However, impurities in concentrated brine will release electrons to form oxygen during the electrolysis process, which is easy to contaminate ion exchange membranes and reduce the purity of the produced chlorine. Therefore, it is necessary to achieve SO4 2- Efficient and selective separation is a scientific problem that needs to be solved urgently.

[0003] Nanofiltration membrane separation technology, as a membrane technology for separating monovalent and polyvalent ions, has become a promising green and environmentally friendly technology. Among them, thin film composite nanofiltration membrane (TFC-NF) consists of a porous support layer base membrane and an ultra-thin active separation layer. It has the advantages of high separation efficiency, stable structure, and easy preparation, and is widely used in seawater softening, lithium extraction from sea brine, and desulfurization in the chlor-alkali industry. However, traditional commercial nanofiltration membranes are usually suitable for the separation of salt water with lower concentrations (500–2000 ppm). When used in high-salt solutions, the following problems will occur: (1) Severe concentration polarization causes a decrease in the permeability flux and separation selectivity of the nanofiltration membrane; (2) It is susceptible to irreversible membrane fouling caused by inorganic salts, organic compounds, and biological adhesion; (3) Because the framework structure of its active separation layer is made of polyamide, it is susceptible to H + The attack causes structural deformation, which makes it difficult to regenerate the membrane after acid washing after membrane fouling. These problems limit the practical application of nanofiltration membranes in the field of high-salt solution separation. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art. In view of the technical bottlenecks of poor anti-fouling and easy acid hydrolysis of traditional commercial nanofiltration membranes, as well as the application difficulties of both reduced permeate flux and separation selectivity when used for concentrated brine separation, a method for preparing an anti-fouling and acid-resistant nanofiltration membrane for use in high-salt water is provided. The prepared nanofiltration membrane exhibits excellent anti-fouling and acid-resistant properties.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] In one aspect, the present invention provides a method for preparing a fouling-resistant and acid-resistant nanofiltration membrane for use in high-salt water, comprising:

[0007] Using the ultrafiltration basement membrane as the substrate, the aqueous solution is infiltrated into the basement membrane with the help of pressure, and the sulfonated two-dimensional porous material (C OFs-SO3H) is completely anchored on the surface of the basement membrane to form an aqueous functional layer, thereby obtaining an ultrafiltration basement membrane with an aqueous functional layer; this step can accurately control the loading amount of functional COFs by the volume of the aqueous solution. The volume of the aqueous solution is between 5 and 30 mL, and the loading amount of functional COFs is controlled to be between 4 and 24 μg cm -2 between.

[0008] The oil phase solution is poured onto the surface of the ultrafiltration base membrane with the water phase functional layer to carry out an interfacial polymerization reaction, and the interfacial reaction time is controlled to be 30 to 120 seconds; the surface is rinsed with a n-hexane solution, and placed in an oven for heat treatment at 60 to 80° C. for 1 to 5 minutes, taken out, and an anti-fouling and acid-resistant nanofiltration membrane is obtained, which is stored in water;

[0009] The preparation method of the ultrafiltration basement membrane is as follows: 10-18wt% of polysulfone, 7.5-8.5wt% of polyethylene glycol 400, 0.05-0.2wt% of dopamine hydrochloride and 73.3-82.45wt% of NN dimethylformamide are weighed in a stoppered conical bottle and sealed, magnetically stirred at 300-500r / min for 12-24h in an oil bath at 60-85°C, and then allowed to stand at room temperature for degassing for 20-25h to obtain a uniform and transparent casting solution; adjusting the scraper thickness to 10-50μm, using water as a coagulation bath, and preparing the ultrafiltration basement membrane by a non-solvent induced phase separation method;

[0010] The preparation method of the aqueous phase solution is: exfoliating the sulfonated two-dimensional porous material (COFs-SO3H) into 20-100nm nanosheets, uniformly dispersing them in an aqueous solution containing 0.5-2wt% piperazine and 0.05-0.2wt% dopamine to obtain an aqueous phase solution.

[0011] Furthermore, the oil phase solution is a 0.05-0.2 wt % n-hexane solution of trimesoyl chloride.

[0012] Furthermore, the preparation method of the sulfonated two-dimensional porous material (COFs-SO3H) is as follows: under a nitrogen atmosphere, 1,3,5-triformyl chloroglucitol and 2,5-diaminobenzenesulfonic acid in a molar ratio of 2:3 and a mixed solvent of mesitylene and 1,4-dioxane in a volume ratio of 1:1 to 4:1 are added to a reactor, and after ultrasonic dispersion for 10 to 20 minutes, the mixture is sealed and placed in an oven at 115 to 130°C for reaction for 48 to 72 hours; a red solid is then filtered to obtain a red solid, which is fully washed with 1,4-dioxane, and the powder is solvent exchanged with acetone, and vacuum dried at 110 to 130°C to obtain a powdered sulfonated two-dimensional porous material (COFs-SO3H).

[0013] Furthermore, the vacuum drying temperature is 110-130° C., and the drying time is 10-14 hours.

[0014] The sulfonated two-dimensional porous material (COFs-SO3H), piperazine, and dopamine in the aqueous solution contain primary or secondary amine groups, which can react with the acyl chloride groups in the trimesoyl chloride in the oil phase to form a network structure of the active separation layer. Among them, the sulfonated two-dimensional porous material (COFs-SO3H) can provide an acid-resistant skeleton structure and sulfonic acid-resistant groups in situ, thereby regulating the surface charge properties of the functional layer; the polydopamine formed by the oxidative self-polymerization of dopamine regulates the hydrophilicity of the functional layer, and the polydopamine and piperazine regulate the aggregation rate of polydopamine through the Michael addition reaction and the Schiff base reaction, while the sulfonated two-dimensional porous material (COFs-SO3H) and dopamine synergistically slow down the diffusion rate of piperazine molecules into the oil phase and the interface reaction rate, thereby regulating the micro-nano structure of the functional active separation layer.

[0015] Furthermore, the sulfonated two-dimensional porous material (COFs-SO3H) is peeled into 40-80nm nanosheets. When the size of the nanosheet is higher than 80nm, it is easy to agglomerate, resulting in uneven dispersion of the aqueous phase, and then the active separation layer formed by interfacial polymerization is prone to form defective pores; when it is lower than 20nm, some nanosheets will not be completely anchored to the surface of the substrate membrane, making it difficult to accurately control the loading amount of COFs.

[0016] Furthermore, the concentration of the sulfonated two-dimensional porous material is 0.009-0.011 mg / mL.

[0017] Furthermore, the concentration of piperazine in the aqueous phase solution is 0.05-1.0 wt %. A piperazine concentration higher than 2 wt % will result in an excessively fast diffusion rate of the aqueous phase monomer during the interfacial polymerization film-forming process, resulting in a relatively large roughness of the active separation layer and easy contamination; a piperazine concentration lower than 0.5 wt % will result in a low cross-linking degree of the active separation layer and a reduced separation selectivity.

[0018] Furthermore, the concentration of dopamine in the aqueous solution is 0.1-0.15 wt%. When the concentration of dopamine is higher than 0.2 wt%, its oxidative self-polymerization reaction is aggravated and polydopamine with larger particle size is easily formed; when the concentration is lower than 0.05 wt%, the effect of participating in the construction and hydrophilic modification of the active separation layer is not obvious.

[0019] Furthermore, the ultrafiltration base membrane can be replaced by a commercial polysulfone membrane.

[0020] Furthermore, the concentration of the high salt water is 3 to 30 g / L sodium sulfate solution.

[0021] The advantages and positive effects of the present invention are:

[0022] 1. The present invention uses a structurally stable sulfonated two-dimensional porous covalent organic framework material (COFs-SO3H) as a functional material. In the film-forming process of interfacial polymerization, dopamine and piperazine are coordinated to participate in the construction of an active separation layer network structure through the amide reaction of the amino group and the acyl chloride group, and sulfonic acid-resistant groups and hydrophilic functional groups are provided in situ. The three synergistically regulate the diffusion rate of the aqueous phase monomer to the oil phase and the interfacial reaction rate, and then regulate the micro-nano structure of the functional active separation layer to form a new functional nanofiltration membrane. In the process of concentrated brine separation, the membrane shows a simultaneous improvement in the permeation flux and the water-salt separation selectivity, and exhibits excellent anti-fouling and acid resistance.

[0023] 2. The method for preparing a novel functional nanofiltration membrane of the present invention can be extended to the preparation of acid-resistant and anti-fouling functional reverse osmosis and forward osmosis membranes. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM morphology image of the sulfonated two-dimensional porous material prepared in Example 1;

[0025] Figure 2 This is a TEM morphology image of the sulfonated two-dimensional porous material nanosheet prepared in Example 1;

[0026] Figure 3 This is the infrared spectrum of the sulfonated two-dimensional porous material nanosheet prepared in Example 1;

[0027] Figure 4 This is a SEM morphology image of the anti-fouling and acid-resistant nanofiltration membrane prepared in Example 1;

[0028] Figure 5 This is a graph showing the separation performance of the anti-fouling and acid-resistant nanofiltration membrane prepared in Example 1 for 0-30 g / L Na2SO4 aqueous solution;

[0029] Figure 6 This is a graph showing the antibacterial performance of the antifouling and acid-resistant nanofiltration membrane prepared in Example 1 against Escherichia coli;

[0030] Figure 7 This is a graph showing the antibacterial performance of the anti-fouling and acid-resistant nanofiltration membrane prepared in Example 1 against Staphylococcus aureus. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0032] Example 1

[0033] A method for preparing a fouling-resistant and acid-resistant nanofiltration membrane for high-salt water, comprising:

[0034] (1) The preparation method of the ultrafiltration basement membrane is as follows: 14 wt% of polysulfone, 4008 wt% of polyethylene glycol, 0.1 wt% of dopamine hydrochloride and 77.9 wt% of N-N-dimethylformamide are weighed in a stoppered conical flask and sealed, and magnetically stirred at 400 r / min for 24 h in an 80° C. oil bath, and then allowed to stand at room temperature for 24 h for degassing to obtain a uniform and transparent casting solution; the scraper thickness is adjusted to 30 μm, water is used as a coagulation bath, and the ultrafiltration basement membrane is prepared by a non-solvent induced phase separation method;

[0035] (2) The preparation method of the aqueous phase solution is:

[0036] Preparation of sulfonated two-dimensional porous material (COFs-SO3H): Under a nitrogen atmosphere, 0.3 mmol of 1,3,5-triformyl chloroglucitol, 0.45 mmol of 2,5-diaminobenzenesulfonic acid and 3 mL of a mixed solvent of mesitylene and 1,4-dioxane in a volume ratio of 4:1 were added to a reactor, and after ultrasonic dispersion for 10 min, the mixture was sealed and placed in an oven at 120°C for reaction for 72 h; a red solid was then filtered to obtain a red solid, which was thoroughly washed with 1,4-dioxane, and the powder was solvent exchanged with acetone for 6 times, and dried in a vacuum drying oven at 120°C for 12 h to obtain a powdered sulfonated two-dimensional porous material (COFs-SO3H).

[0037] 1 mg of the sulfonated two-dimensional porous material was weighed and dispersed in 100 mL of pure water, and the mixture was peeled off by an ultrasonic crusher at 600 W for 2 h to form a nanosheet aqueous solution with an average particle size of 60 nm. 10 mL of the nanosheet aqueous solution was transferred and 1.0 wt % of piperazine and 0.1 wt % of dopamine were dissolved to obtain an aqueous phase solution.

[0038] (3) The oil phase solution is prepared by dissolving 0.1% trimesoyl chloride in n-hexane solution and mixing to obtain an oil phase solution;

[0039] (4) Using the ultrafiltration base membrane described in step (1) as the base, the aqueous solution prepared in step (2) is pressure-assisted to infiltrate the ultrafiltration base membrane, and the sulfonated two-dimensional porous material (COFs-SO3H) is completely anchored on the ultrafiltration base membrane with an area of ​​12.56 cm 2 forming a water phase functional layer on the surface of the ultrafiltration basement membrane to obtain an ultrafiltration basement membrane having a water phase functional layer;

[0040] (5) pouring the oil phase solution prepared in step (3) onto the membrane surface of the ultrafiltration base membrane with the water phase functional layer obtained in step (4) to carry out an interfacial polymerization reaction, controlling the interfacial reaction time to be 60 s, rinsing the membrane surface with n-hexane solution, and placing it in an oven for heat treatment at 80°C for 1 min, taking it out to obtain an anti-fouling and acid-resistant nanofiltration membrane, and storing it in water.

[0041] The sulfonated two-dimensional porous material prepared in Example 1 was characterized. Figure 1 This is the SEM morphology of the sulfonated two-dimensional porous material; Figure 2 TEM morphology of sulfonated two-dimensional porous material nanosheets; Figure 3 This is the infrared spectrum of sulfonated two-dimensional porous material nanosheets.

[0042] The SEM morphology of the anti-fouling and acid-resistant nanofiltration membrane prepared in Example 1 is as follows: Figure 4 shown.

[0043] Example 2

[0044] A method for preparing a fouling-resistant and acid-resistant nanofiltration membrane for high-salt water, comprising:

[0045] (1) The preparation method of the ultrafiltration basement membrane is as follows: 18 wt% of polysulfone, 8 wt% of polyethylene glycol 400, 0.2 wt% of dopamine hydrochloride and 73.8 wt% of N-N-dimethylformamide are weighed in a stoppered conical flask and sealed, and magnetically stirred at 400 r / min for 24 h in an 80° C. oil bath, and then allowed to stand at room temperature for 24 h for degassing to obtain a uniform and transparent casting solution; the scraper thickness is adjusted to 25 μm, and water is used as a coagulation bath to prepare the ultrafiltration basement membrane by a non-solvent induced phase separation method;

[0046] (2) The preparation method of the aqueous phase solution is:

[0047] Preparation of sulfonated two-dimensional porous material (COFs-SO3H): ① Under a nitrogen atmosphere, 1,3,5-triformyl chloroglucitol (0.3 mmol), 2,5-diaminobenzenesulfonic acid (0.45 mmol) and a mixed solvent of mesitylene and 1,4-dioxane in a volume ratio of 4:1 (3 mL) were added to a reactor, ultrasonically dispersed for 10 min, and then sealed and placed in an oven at 120°C for reaction for 72 h; then a red solid was filtered to obtain a red solid, which was thoroughly washed with 1,4-dioxane, and the powder was solvent exchanged with acetone for 6 times, and dried in a vacuum drying oven at 120°C for 12 h to obtain a powdered sulfonated two-dimensional porous material (COFs-SO3H).

[0048] 1 mg of the sulfonated two-dimensional porous material was dispersed in 150 mL of pure water, and the material was peeled off by an ultrasonic crusher (600 W) for 1 h to form a nanosheet aqueous solution with an average particle size of 80 nm. 30 mL of the nanosheet aqueous solution was transferred, and 1.0 wt % of piperazine and 0.1 wt % of dopamine were dissolved to obtain an aqueous phase solution;

[0049] (3) The oil phase solution is prepared by dissolving 0.15% trimesoyl chloride in n-hexane solution and mixing to obtain an oil phase solution;

[0050] (4) Using the ultrafiltration base membrane described in step (1) as the base, the aqueous solution prepared in step (2) is pressure-assisted to infiltrate the ultrafiltration base membrane, and the sulfonated two-dimensional porous material (COFs-SO3H) is completely anchored on the ultrafiltration base membrane with an area of ​​12.56 cm 2 forming a water phase functional layer on the surface of the ultrafiltration basement membrane to obtain an ultrafiltration basement membrane having a water phase functional layer;

[0051] (5) pouring the oil phase solution prepared in step (3) onto the membrane surface of the ultrafiltration base membrane with the water phase functional layer obtained in step (4) to carry out an interfacial polymerization reaction, controlling the interfacial reaction time to be 60 s, rinsing the membrane surface with n-hexane solution, and placing it in an oven for heat treatment at 80°C for 1 min, taking it out to obtain an anti-fouling and acid-resistant nanofiltration membrane, and storing it in water.

[0052] Comparative Example 1

[0053] The difference from Example 1 is that in the aqueous solution in step (2), no sulfonated two-dimensional porous material (COFs-SO3H) and dopamine are used.

[0054] Comparative Example 2

[0055] The difference from Example 1 is that no sulfonated two-dimensional porous material (COFs-SO3H) is used in the aqueous solution in step (2).

[0056] Comparative Example 3

[0057] The difference from Example 1 is that dopamine is not used in the aqueous solution in step (2).

[0058] Performance Testing

[0059] Test method for the separation performance of anti-fouling and acid-resistant nanofiltration membrane in high salt water: m 12.56cm 2 The membrane sample is fixed in the membrane pool of the cross-flow membrane separation device, and a high-salt aqueous solution of sodium sulfate with a concentration of 0 to 30 g / L is used as the feed liquid. After the membrane is compacted at 0.8 MPa, the permeate is collected at ΔP = 0.6 MPa, and the collection time (Δt) and the permeate volume (Q) are recorded. The permeate flux of the anti-fouling and acid-resistant nanofiltration membrane is calculated according to formula (1), and the barium sulfate weight method is used to calculate the retention rate of Na2SO4 of the anti-fouling and acid-resistant nanofiltration membrane according to formula (2). Wherein, Δπ represents the osmotic pressure of the feed liquid, C f and C p Represent the concentration of sodium sulfate in the feed liquid and the permeate respectively; the water-salt separation selectivity α of the anti-fouling and acid-resistant nanofiltration membrane is calculated according to formula (3).

[0060]

[0061]

[0062]

[0063] Antibacterial test method: The "inhibition zone method" was used to test the antibacterial performance of the acid-resistant and anti-fouling nanofiltration membrane. The experimental equipment (culture dishes, inoculation loops, tweezers, knives, etc.) used in the experiment were sterilized in a high-pressure steam cooker at 103.4kPa and 120°C for 2h. A membrane sample with a diameter of 6.00mm was placed on a solid Luria-Bertani (LB) medium, and two microorganisms, Escherichia coli (E.coli., CGMCC12340) and Staphylococcus aureus (SAU, ATCC6538), were coated on the LB medium. After culturing in an intelligent constant temperature oscillator at 37°C for 24h, the size of the antibacterial zone around the acid-resistant and anti-fouling nanofiltration membrane was observed and measured. The larger the antibacterial zone, the better the antibacterial effect.

[0064] Acid resistance test method: After the prepared anti-fouling and acid-resistant nanofiltration membrane is soaked in 4.9% sulfuric acid solution for 30 days, it is fully washed with deionized water and fixed in the membrane pool of the cross-flow membrane separation device. The permeation flux and retention rate are tested with a sodium sulfate aqueous solution with a concentration of 3g / L as the feed liquid. The acid resistance of the nanofiltration membrane is evaluated by comparing the changes in the permeation flux and retention rate of the nanofiltration membrane before and after soaking in sulfuric acid solution. If the permeation flux and sodium sulfate retention rate of the nanofiltration membrane are almost unchanged after acid soaking, it indicates that the acid resistance of the nanofiltration membrane is good.

[0065] The above test results are as follows Figures 5 to 7 shown.

[0066] The above test results are shown in Table 1.

[0067] Table 1 Test results of anti-fouling and acid-resistant nanofiltration membranes prepared in Examples 1 to 2 and Comparative Examples 1 to 3

[0068]

[0069] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a fouling-resistant and acid-resistant nanofiltration membrane for high-salt water, characterized in that: Taking the ultrafiltration basement membrane as the base, the aqueous phase solution is infiltrated into the ultrafiltration basement membrane with the aid of pressure to obtain the ultrafiltration basement membrane with the aqueous phase functional layer; the oil phase solution is poured onto the membrane surface of the ultrafiltration basement membrane with the aqueous phase functional layer to carry out the interfacial polymerization reaction, the interfacial reaction time is controlled to be 30 to 120 seconds, the membrane surface is rinsed with n-hexane solution, and the membrane is placed in an oven for heat treatment at 60 to 80° C. for 1 to 5 minutes, and then taken out to obtain the anti-fouling and acid-resistant nanofiltration membrane, which is stored in water; The preparation method of the ultrafiltration basement membrane is as follows: 10-18wt% of polysulfone, 7.5-8.5wt% of polyethylene glycol 400, 0.05-0.2wt% of dopamine hydrochloride and 73.3-82.45wt% of NN dimethylformamide are weighed in a stoppered conical bottle and sealed, magnetically stirred at 300-500r / min for 12-24h in an oil bath at 60-85°C, and then allowed to stand at room temperature for degassing for 20-25h to obtain a uniform and transparent casting solution; adjusting the scraper thickness to 10-50μm, using water as a coagulation bath, and preparing the ultrafiltration basement membrane by a non-solvent induced phase separation method; The preparation method of the aqueous phase solution is: peeling the sulfonated two-dimensional porous material into 20-100nm nanosheets, uniformly dispersing them in an aqueous solution containing 0.5-2wt% piperazine and 0.05-0.2wt% dopamine to obtain an aqueous phase solution.

2. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The oil phase solution is a 0.05-0.2 wt % n-hexane solution of trimesoyl chloride.

3. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The preparation method of the sulfonated two-dimensional porous material is as follows: under a nitrogen atmosphere, 1,3,5-triformyl chloroglucitol and 2,5-diaminobenzenesulfonic acid in a molar ratio of 2:3 and a mixed solvent of mesitylene and 1,4-dioxane in a volume ratio of 1:1 to 4:1 are added into a reaction kettle, and after ultrasonic dispersion for 10 to 20 minutes, the mixture is sealed and placed in an oven at 115 to 130° C. for reaction for 48 to 72 hours; a red solid is then filtered to obtain a red solid, which is fully washed with 1,4-dioxane, and the powder is subjected to solvent exchange with acetone, and vacuum dried to obtain a powdery sulfonated two-dimensional porous material.

4. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The sulfonated two-dimensional porous material is exfoliated into nanosheets of 40 to 80 nm.

5. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The concentration of the sulfonated two-dimensional porous material in the aqueous solution is 0.009-0.011 mg / mL.

6. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The concentration of piperazine in the aqueous phase solution is 0.10-0.15 wt %.

7. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The concentration of dopamine in the aqueous solution is 0.10-0.15 wt %.

8. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to claim 1, characterized in that: The ultrafiltration base membrane may use a commercially available polysulfone membrane.

9. The method for preparing the anti-fouling and acid-resistant nanofiltration membrane for high-salt water according to any one of claims 1 to 8, characterized in that: The concentration of the high salt water is 3-30 g / L.

Citation Information

Cited By

  • High-performance mesoporous silica / polysulfonamide acid-resistant nanofiltration membrane as well as preparation method and application thereof