Preparation method of iron-site-doped LaFeO3 perovskite material and application of iron-site-doped LaFeO3 perovskite material in phosphorus removal field
By mixing lanthanum salts, iron salts and doped metal salts in water, and using a one-step drying and one-step firing method to prepare iron site-doped LaFeO3 perovskite materials, it solves the cumbersome preparation process and limited phosphorus removal performance in the existing technology. problems, achieving simplified processes and improved performance, and are suitable for industrial production and various applications.
Patent Information
- Application Number
- CN202411091119.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-22
AI Technical Summary
The preparation process of existing iron-site-doped LaFeO3 perovskite materials is cumbersome and time-consuming, making it unsuitable for large-scale industrial production. Moreover, the perovskite structure requires high process conditions, resulting in limited phosphorus removal performance of the material.
Iron site-doped LaFeO3 perovskite materials are prepared by directly mixing lanthanum salts, iron salts and doped metal salts in water, followed by one-step drying and one-step firing. This method simplifies the operating steps, controls the molar ratio and concentration, and is suitable for many applications. Doped with a variety of metals, it has wider adaptability.
The preparation time is greatly shortened, the synthesis efficiency is improved, and industrial production is achieved. The phosphorus removal performance of the obtained material is improved, and the applicable pH range is wider, and the application range is wider.
Smart Images

Figure CN118807680A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of water treatment and specifically relates to an iron-site doped LaFeO 3 Preparation method of perovskite material and its application in phosphorus removal field. Background Art
[0002] Urban domestic sewage is large in volume and has stable water quality. After deep treatment, it can be used as an important water source for replenishment. However, traditional biological treatment processes often have poor phosphorus removal effects and require deep treatment of the effluent. Adsorption technology has the advantages of simple operation, low energy consumption and stable operation. It can also achieve deep reduction of phosphates in sewage and recovery of phosphorus resources at the same time, but the research and development of phosphorus adsorption materials is the key.
[0003] LaFeO 3 Perovskite has a stable crystal structure, and metal ions are not easily dissolved, so it is often used for adsorption or catalytic materials. 3 Perovskite is easy to form a crystal defect structure by doping and replacing the iron site, which can achieve good regulation of the material's acid-base site, specific surface area, zero potential point, etc., thereby improving the material's phosphorus removal performance and has great application potential and value in the field of water treatment. However, the formation process of the perovskite structure requires high process conditions, resulting in the existing iron site doping LaFeO 3 The preparation process of perovskite materials is complicated and time-consuming, which is not conducive to large-scale industrial production.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide an iron-site doped LaFeO 3 A method for preparing perovskite materials. The method greatly simplifies the operation steps while ensuring the formation of perovskite, saves time and energy, and is conducive to industrial production. At the same time, the method is also suitable for multiple metal doping and has a wider application range. The obtained material is suitable for a wider pH range and has better adaptability.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides an iron-site doped LaFeO 3 The method for preparing the perovskite material comprises the following steps: S1, adding lanthanum salt, iron salt, doped metal salt and citric acid into water and stirring; S2, drying the mixture obtained in step S1 in one step and grinding it into powder; S3, sintering the powder obtained in step S2 in one step to obtain the iron-site doped LaFeO 3 Perovskite materials.
[0007] In the above preparation method, in step S1, the lanthanum salt is selected from at least one of lanthanum nitrate, lanthanum chloride, and lanthanum acetate; preferably lanthanum nitrate.
[0008] In the above preparation method, in step S1, the iron salt is selected from at least one of iron nitrate, iron chloride, and iron acetate, and preferably iron nitrate.
[0009] In the above preparation method, in step S1, the doped metal is selected from at least one of aluminum, copper, manganese, cobalt, and zirconium. The doped metal salt is selected from nitrates.
[0010] In the above preparation method, in step S1, the molar ratio of the lanthanum salt, the iron salt, the doped metal salt, and the citric acid ranges from 1:1:(3 - 6).
[0011] In the above preparation method, in step S1, the molar ratio of the iron salt to the doped metal salt is x:(1 - x), where 0.5 < x ≤ 1.
[0012] In the above preparation method, in step S1, the concentration of the lanthanum salt in water ranges from 0.1 - 1 mol / L, specifically such as 0.1 - 0.2 mol / L.
[0013] According to the specific embodiments of the present invention, when the metal in the doped metal salt is aluminum and zirconium, 0.8 < x < 1; in addition, it is found through research that when x = 0.7, the LaFeO doped with aluminum 3 material cannot obtain a pure - phase perovskite structure; when the metal in the doped metal salt is copper, manganese, or cobalt, 0.5 < x < 1. Research shows that controlling iron within this range can avoid the generation of impurity phases caused by excessive doping and is beneficial to the preparation of pure - phase LaFeO without impurity peaks 3 perovskite.
[0014] In the above preparation method, in step S1, the conditions for stirring are: at normal temperature of 20 - 30 °C, preferably 25 °C, and the time range is 4 - 6 h, preferably 4 h.
[0015] In the above preparation method, in step S2, the conditions for drying are: the temperature range is 80 - 120 °C, preferably 80 °C, and the time range is 6 - 18 h, preferably 12 h.
[0016] In the above preparation method, in step S2, the particle size of the powder is not less than 80 mesh, preferably 100 mesh.
[0017] In the above preparation method, in step S3, the conditions for firing are: the temperature range is 700 - 900 °C, preferably 700 °C, the time range is 2 - 5 h, and the heating rate is 5 - 15 °C / min.
[0018] In a second aspect, the present invention provides the iron-site doped LaFeO obtained by the above preparation method. 3 Perovskite materials.
[0019] The iron site doped LaFeO3 perovskite material is LaFe 0.9 Al 0.1 O 3 、LaFe 0.8 Al 0.2 O 3 、LaFe 0.7 Cu 0.3 O 3 、LaFe 0.7 Mn 0.3 O 3 、LaFe 0.9 Zr 0.1 O 3 、LaFe 0.7 Co 0.3 O 3 .
[0020] In a third aspect, the present invention provides an adsorbent, comprising the above-mentioned iron site-doped LaFeO 3 Perovskite materials.
[0021] In a fourth aspect, the present invention provides the above-mentioned iron site doped LaFeO 3 Application of perovskite materials or adsorbents in water treatment, environmental catalysis, and optoelectronic materials.
[0022] Compared with the prior art, the present invention has the following beneficial effects: The present invention directly mixes the materials in water, and by controlling the amount relationship of the materials and their concentrations in water, reaction conditions and other factors, the reaction between the lanthanum salt, the iron salt and the doped metal salt is promoted to be more complete, and the generation of other oxides is avoided, thereby simplifying the subsequent process, achieving one-step drying and one-step firing, greatly shortening the preparation time, improving the synthesis efficiency, and being conducive to realizing industrial production; at the same time, the method is applicable to multiple metal doping, so that the application range of the obtained perovskite material is wider; in addition, under the premise of ensuring the adsorption performance, the iron site doped LaFeO prepared by the present invention 3 The pH range of perovskite materials is wider and their application range is wider. 3 Improvements in the preparation process of perovskite materials have achieved multiple unexpected technical effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is LaFe 1-x B x O 3(B=Al, Cu, Mn, Co, Zr) adsorbent XRD patterns.
[0024] Figure 2 It is LaFe 1-x B x O 3 Scanning energy spectrum of (B=Al, Cu, Mn, Co, Zr) adsorbent.
[0025] Figure 3 It is LaFe 1-x B x O 3 (B=Al, Cu, Mn, Co, Zr) Phosphorus removal performance of adsorbent (initial phosphorus concentration=2mg / L; dosage=0.3g / L; adsorption time=4h). DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.
[0027] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0028] Unless otherwise specified, the reagents, materials, instruments, etc. used in the following examples can be obtained from commercial sources.
[0029] Example 1: LaFe 0.9 Al 0.1 O 3 Preparation of perovskite materials Here are the steps: (1) 0.02 mol of lanthanum acetate hydrate, 0.018 mol of ferric nitrate nonahydrate, 0.002 mol of aluminum chloride and 0.06 mol of hydrated citric acid were placed in 150 mL of deionized water, and stirred at room temperature for 4 h using a magnetic stirrer to mix evenly; (2) drying the mixture obtained in step (1) in an oven at 80° C. for 12 h, and grinding to obtain a powder with a size greater than 100 mesh; (3) The powder obtained in step (2) was calcined in a muffle furnace at 700°C for 2 h at a heating rate of 10°C / min to obtain LaFe 0.9 Al 0.1 O 3 Perovskite materials.
[0030] Example 2 The method is the same as in Example 1, except that 0.002 mol of aluminum chloride is replaced by 0.002 mol of zirconium nitrate to obtain LaFe 0.9 Zr 0.1 O 3 Material.
[0031] Example 3 The method is the same as that of Example 1, except that 0.018 mol of ferric nitrate nonahydrate and 0.002 mol of aluminum chloride are replaced with 0.014 mol of ferric nitrate nonahydrate and 0.006 mol of copper nitrate to obtain LaFe 0.7 Cu 0.3 O 3 Material.
[0032] Example 4 The method is the same as that of Example 1, except that 0.018 mol of ferric nitrate nonahydrate and 0.002 mol of aluminum chloride are replaced by 0.014 mol of ferric nitrate nonahydrate and 0.006 mol of manganese nitrate to obtain LaFe 0.7 Mn 0.3 O 3 Material.
[0033] Example 5 The method is the same as that of Example 1, except that 0.018 mol of ferric nitrate nonahydrate and 0.002 mol of aluminum chloride are replaced with 0.014 mol of ferric nitrate nonahydrate and 0.006 mol of cobalt nitrate to obtain LaFe 0.7 Co 0.3 O 3 Material.
[0034] Comparative Example 1 The method is the same as that in Example 1, except that no aluminum salt is added in step 1, and the amount of lanthanum salt and iron salt added to the mixed solution is 0.02 mol, to obtain LaFeO 3 Material.
[0035] Comparative Example 2 The method is the same as that in Example 1, except that no aluminum salt is added in step 1, the dosage of lanthanum salt and iron salt in the mixed solution is 0.02 mol, the muffle furnace calcination temperature is 400° C., and the results show that no perovskite structure is formed.
[0036] Test Case 1. X-ray diffraction (XRD) analysis X-ray diffraction (XRD) analysis was performed on the adsorbent materials obtained in Examples 1-5 and Comparative Example 1 to analyze the crystal structure of the adsorbent materials. The analysis results are shown in Figure 1 .
[0037] Figure 1 LaFeO doped with Al, Cu, Mn, Co and Zr 3 XRD pattern of perovskite, Figure 1 It can be seen that the material has a 2θ value of 22.6 o , 32.2o , 39.7 o , 46.2 o , 57.4 o and 67.4 o Characteristic diffraction peaks appear near, corresponding to LaFeO 3 The typical crystal plane characteristic diffraction peaks of perovskite (COD#1526450) (110), (112), (202), (220), (312) and (224) are absent, and there are no other metal oxide peaks. The results show that pure LaFeO was successfully prepared. 3 .
[0038] At the same time, LaFeO doped with different metals such as Al, Cu, Mn, Co and Zr was used. 3 After doping, LaFeO appeared in all five metal composites. 3 The characteristic peaks of perovskite (COD#1526450) are shifted to a certain extent, which may be due to metal doping into LaFeO 3 In crystal structure.
[0039] 2. Plasma emission spectroscopy (XPS) analysis The adsorption materials prepared in Examples 1-5 and Comparative Example 1 were subjected to XPS analysis to analyze the elemental composition of the adsorption materials. The analysis results are shown in Figure 2 .
[0040] Figure 2 LaFeO doped with Al, Cu, Mn, Co and Zr 3 XPS spectrum of perovskite. Figure 2 It can be seen that LaFeO 3 There are La, Fe and O elements on the surface. After Al, Cu, Mn, Co and Zr metal doping, the corresponding metal element new peaks appear on the spectrum, and new peaks of Al, Cu, Mn, Co and Zr appear, and no new substances are generated (see Figure 1 ), indicating that Al, Cu, Mn, Co and Zr were successfully doped into LaFeO 3 In the lattice.
[0041] 3. Nitrogen adsorption and desorption analysis The adsorption materials prepared in Examples 1-5 and Comparative Example 1 were subjected to nitrogen adsorption-desorption analysis to analyze the specific surface area, average pore volume and pore diameter of the adsorption materials. The analysis results are shown in Table 1.
[0042] Table 1 LaFe 1-x B x O 3 (B=Al, Cu, Mn, Co, Zr) Physical properties
[0043] As shown in Table 1, metal doping increases the specific surface area and average pore volume of the adsorbent. 1-x B x O 3 Specific surface area is 8.8-20.5 m 2 / g; except for Zr doping, the addition of other metals reduces the average pore size of the material, which may be due to the larger ionic radius Zr 4+ Replace Fe 3+ The site causes.
[0044] 4. Phosphorus removal performance Phosphorus removal experiments were conducted on the adsorption materials prepared in Examples 1-5 and Comparative Example 1 to analyze the phosphorus removal performance of the adsorbents.
[0045] The specific steps of the phosphorus removal experiment are as follows: 0.3 g / L adsorbent was added to 2 mg / L phosphorus solution, the solution pH was not adjusted, the solution pH was 5.8, adsorption was carried out for 4 h, and the phosphate concentration in the aqueous solution after adsorption was determined by ammonium molybdate spectrophotometry.
[0046] The analysis results are shown in Figure 3 .
[0047] Figure 3 LaFeO doped with Al, Cu, Mn, Co and Zr 3 Phosphorus removal performance of perovskite. Figure 3 It can be seen that the order of phosphate removal rate from large to small is LaFe 0.9 Al 0.1 O 3 >LaFe 0.7 Cu 0.3 O 3 >LaFe 0.7 Mn 0.3 O 3 >LaFe 0.9 Zr 0.1 O 3 >LaFe 0.7 Co 0.3 O 3 >LaFeO 3 Compared with pure LaFeO 3 , Al, Cu, Mn, Co and Zr metal doping can significantly improve the phosphate removal rate, and the phosphorus removal rate increased by 12.6-61.3%. Al doping has the best phosphorus removal effect.
[0048] Example 6: LaFe 0.8 Al 0.2 O 3 Preparation of perovskite materials The method is the same as that of Example 1, except that 0.018 mol of ferric nitrate nonahydrate and 0.002 mol of aluminum chloride are replaced by 0.016 mol of ferric nitrate nonahydrate and 0.004 mol of aluminum chloride to obtain LaFe 0.8 Al 0.2 O 3 Perovskite materials.
[0049] The above phosphorus removal test was used for testing, and the results showed that 0.3g / L LaFe 0.8 Al 0.2 O 3 The perovskite material treated 2 mg / L phosphorus solution, without adjusting the solution pH, the phosphate removal rate could reach 98% in 4 hours; by adjusting the initial pH of the phosphorus solution, the results showed that LaFe 0.8 Al 0.2 O 3 The material has a wide pH range. When the initial pH is 4-9, 0.3g / L LaFe 0.8 Al 0.2 O 3 The material treated 2mg / L phosphorus solution, the phosphorus removal rate remained stable, the phosphate removal rate fluctuated between 98% and 99%, and at a pH of 10, the phosphate removal rate could reach 85%. 0.8 Al 0.2 O 3 Material treatment 10-80mg / L phosphorus solution, determination of equilibrium phosphate concentration, LaFe 0.8 Al 0.2 O 3 The phosphorus saturation adsorption capacity of the material is 53 mg / g. 0.8 Al 0.2 O 3 The phosphorus removal performance of the perovskite material is better than that of the perovskite material obtained in Examples 1-5.
[0050] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing an iron-site doped LaFeO3 perovskite material, comprising the following steps: S1, adding lanthanum salt, iron salt, doped metal salt and citric acid into water and stirring; S2, drying the mixture obtained in step S1 in one step and grinding it into powder; S3, sintering the powder obtained in step S2 in one step to obtain the iron-site doped LaFeO3 perovskite material.
2. The preparation method according to claim 1, characterized in that: In step S1: The lanthanum salt is selected from at least one of lanthanum nitrate, lanthanum chloride and lanthanum acetate; The iron salt is selected from at least one of ferric nitrate, ferric chloride and ferric acetate; The doping metal is selected from at least one of aluminum, copper, manganese, cobalt and zirconium.
3. The preparation method according to claim 1 or 2, characterized in that: In step S1: The molar ratio of the lanthanum salt, the iron salt and the doped metal salt, and the citric acid is in the range of 1:1:(3-6); The molar ratio of the iron salt to the doping metal salt is x: (1-x), 0.5 <x≤1; The concentration range of the lanthanum salt in water is 0.1-1 mol / L.
4. The preparation method according to any one of claims 1 to 3, characterized in that In step S1, the stirring conditions are: room temperature 20-30°C, and time range is 4-6h.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S2, the drying conditions are: temperature range is 80-120°C, time range is 6-18h; The particle size of the powder is not less than 80 meshes.
6. The preparation method according to any one of claims 1 to 5, characterized in that: In step S3, the firing conditions are: temperature range is 700-900°C, time range is 2-5h, and heating rate is 5-15°C / min.
7. The iron-site doped LaFeO3 perovskite material obtained by the preparation method according to any one of claims 1 to 6.
8. The iron-site doped LaFeO3 perovskite material according to claim 7, characterized in that: The iron site doped LaFeO3 perovskite material is LaFe 0.9 Al 0.1 O3、LaFe 0.8 Al 0.2 O3、LaFe 0.7 Cu 0.3 O3、LaFe 0.7 Mn 0.3 O3、LaFe 0.9 Zr 0.1 O3、LaFe 0.7 Co 0.3 O3.
9. An adsorbent comprising the iron-site doped LaFeO3 perovskite material according to claim 7 or 8.
10. Use of the iron-site doped LaFeO3 perovskite material according to claim 7 or 8 or the adsorbent according to claim 9 in the fields of water treatment, environmental catalysis, and photoelectric materials.
Citation Information
Patent Citations
La-Fe-Al composite metal oxide, preparation method and application
CN114225895A