Polyvinyl alcohol spherical microbial carrier as well as preparation method and application thereof

Through the cross-linking reaction of polyvinyl alcohol and sodium alginate, combined with phosphate esterification treatment, the problem of high water solubility of PVA gel beads was solved, and a spherical microbial carrier with low water solubility and high mechanical strength was prepared, which improved the efficiency of wastewater treatment. Processing efficiency and carrier durability.

CN118813596APending Publication Date: 2024-10-22YISHUIYUAN BIOTECHNOLOGY (XIAN) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410821044.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing polyvinyl alcohol (PVA) gel beads have high water solubility, resulting in poor flocculation effect and affecting the efficiency of sewage treatment.

Method used

By cross-linking a mixed solution of polyvinyl alcohol and sodium alginate with a mixed solution of boric acid-calcium chloride to form a stable polymer network structure, and esterifying it in a phosphate solution, a poly(vinyl alcohol) and sodium alginate mixed solution with low water solubility and high mechanical strength was prepared. Vinyl alcohol spherical microbial carrier.

Benefits of technology

It effectively reduces the adhesion and aggregation between carriers, improves the stability and durability of the suspended state, extends the service life, simplifies the separation process, and improves the economy and sustainability of the carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118813596A_ABST
    Figure CN118813596A_ABST
Patent Text Reader

Abstract

The invention discloses a polyvinyl alcohol spherical microbial carrier as well as a preparation method and application thereof, and relates to the technical field of microbial carriers, the method comprises the following steps: adding polyvinyl alcohol and sodium alginate into water to form a polyvinyl alcohol-sodium alginate mixed solution, the mass fraction of the polyvinyl alcohol is 10-11%, and the mass fraction of the sodium alginate is 10-15%; the mass fraction of the sodium alginate is 2%-3%; boric acid and calcium chloride are dissolved in water to form a boric acid-calcium chloride mixed solution, and in the boric acid-calcium chloride mixed solution, the mass fraction of boric acid is 10%-20%, and the mass fraction of calcium chloride is 3%-5%; dropwise adding the polyvinyl alcohol-sodium alginate mixed solution into the boric acid-calcium chloride mixed solution, fully cross-linking, washing with water, and then soaking in a phosphate solution for esterification to obtain the polyvinyl alcohol gel beads. The problems that in the prior art, polyvinyl alcohol gel beads are high in water solubility, the flocculation effect is poor, and the sewage treatment efficiency is affected are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microbial carriers, and more specifically to a polyvinyl alcohol spherical microbial carrier and a preparation method and application thereof. Background Art

[0002] Living cell immobilization technology refers to a biotechnology that uses physical or chemical means to confine living cells to a specific spatial area and inside or on the surface of a carrier material, so that they can be reused while maintaining their activity. Compared with traditional activated sludge treatment methods, living cell immobilization technology can significantly increase the concentration of microorganisms, shorten treatment time, and reduce treatment costs. The protective effect of the carrier makes it difficult for microorganisms to be lost, and their resistance to toxicity and tolerance are significantly increased. Solid-liquid separation is easy and can be reused repeatedly. It is an efficient, low-consumption, and easy-to-operate and manage sewage biological treatment technology that can effectively treat organic wastewater, ammonia-containing wastewater, heavy metal wastewater, and dye wastewater, and has excellent development prospects.

[0003] The key to the technology is to select a suitable microbial carrier. The microbial carrier not only needs to have good biological affinity and a large specific surface area to meet the conditions for microbial growth, but also requires good mechanical properties to resist the impact of hydraulic shear, and also requires appropriate density to achieve a suspended state in water. Polymer materials have low density, high stability, and are easy to mold and process into various shapes, so they are widely used as microbial carrier materials.

[0004] Natural high molecular weight polysaccharides such as sodium alginate, gelatin, and agar have the advantages of wide sources, convenient solidification and low toxicity to microorganisms, but their mechanical strength is low. They are deformed by hydraulic scouring during long-term sewage treatment processes, thus losing their application value. Synthetic polymers such as polyacrylamide (PAM) and photoresin have the advantages of anti-biological decomposition and high mechanical strength, but the polymer molding conditions are relatively severe and often have high toxicity to microorganisms. Polyvinyl alcohol (PVA) has the advantages of good chemical stability, high anti-biological decomposition ability, high mechanical strength, no biological toxicity and low price. It has great potential value in the field of microbial carriers and has quickly become a hot topic of research at home and abroad. However, polyvinyl alcohol needs to be cross-linked to eliminate water solubility before it can be used as a sewage treatment material. Although the existing boric acid cross-linking method is simple in process, the prepared PVA gel beads have been widely used as microbial carrier materials, but the water solubility of PVA gel beads is still high, resulting in poor flocculation effect and affecting treatment efficiency. Summary of the invention

[0005] Based on this, the present invention provides a polyvinyl alcohol spherical microbial carrier and a preparation method and application thereof, so as to solve the problem of high water solubility of PVA gel beads in the prior art.

[0006] The present invention is achieved through the following technical solutions:

[0007] Adding polyvinyl alcohol and sodium alginate into water to form a polyvinyl alcohol-sodium alginate mixed solution, wherein the mass fraction of polyvinyl alcohol is 10%-11%, and the mass fraction of sodium alginate is 2%-3%;

[0008] Dissolving boric acid and calcium chloride in water to form a boric acid-calcium chloride mixed solution, wherein the mass fraction of boric acid is 10%-20%, and the mass fraction of calcium chloride is 3%-5%;

[0009] The polyvinyl alcohol-sodium alginate mixed solution is added dropwise to the boric acid-calcium chloride mixed solution for full cross-linking, then washed with water, and then immersed in a phosphate solution for esterification to obtain polyvinyl alcohol gel beads.

[0010] Preferably, the polyvinyl alcohol is a powdered solid with a particle size of 100 mesh.

[0011] Preferably, the purity of the sodium alginate is greater than or equal to 98% by mass; preferably, the purity of the sodium alginate is 98% by mass.

[0012] Preferably, in the polyvinyl alcohol-sodium alginate mixed solution, the mass fraction of polyvinyl alcohol is 10% and the mass fraction of sodium alginate is 2%.

[0013] Preferably, in the boric acid-calcium chloride mixed solution, the mass fraction of boric acid is 10%, and the mass fraction of calcium chloride is 3%.

[0014] Preferably, the dripping refers to dripping the polyvinyl alcohol-sodium alginate mixed solution into the boric acid-calcium chloride mixed solution at a height of 20 cm using an instrument with a 3 mm diameter nozzle at the end, and the instrument is a peristaltic pump.

[0015] Preferably, the phosphate solution has a concentration of 0.5 M and a pH of 6-7.

[0016] Preferably, the esterification time is greater than or equal to 4 hours.

[0017] Preferably, the preparation method produces polyvinyl alcohol spherical microbial carriers.

[0018] Preferably, the polyvinyl alcohol spherical microorganism carrier is used in living cell immobilization technology.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) When preparing polyvinyl alcohol (PVA) spherical microbial carriers, the cross-linking reaction between sodium alginate and calcium ions is almost instantaneous, so that the droplets quickly generate a smooth and non-sticky surface, thereby preventing the adhesion and aggregation of the small balls, and achieving the purpose of improving the spheroidization of the PVA solution. This surface property effectively prevents the adhesion and aggregation of the small balls. At the same time, the prepared spherical carrier effectively reduces the fluid resistance, so that the energy required for the carrier to maintain a suspended state in the sewage treatment structure is minimized. In addition, the spherical structure also helps to reduce the collision and wear between the carriers, which not only improves the durability of the carrier, but also extends its service life. Since the carriers are independently dispersed and not easy to clog, the separation process after use becomes simple and can be achieved by conventional filtration. The nature of these carriers that can be recycled multiple times further improves their economy and sustainability, providing strong technical support for environmental protection and resource conservation.

[0021] (2) When preparing polyvinyl alcohol (PVA) spherical microbial carriers, boric acid is used as a cross-linking agent, which can effectively form a stable polymer network structure inside the carrier. Through this cross-linking process, not only the mechanical strength and toughness of the carrier are significantly improved, but also its ability to resist hydraulic erosion is enhanced. In addition, by reacting PVA with a phosphate solution for esterification, the water solubility of the carrier material is further reduced, the water resistance of the carrier is effectively improved, its service life is significantly extended, and the application of PVA gel beads in microbial carriers is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is the swelling rate test curve of the present invention;

[0024] Figure 2 This is the mass transfer efficiency test curve of the present invention. DETAILED DESCRIPTION

[0025] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0027] The technical solution is as follows:

[0028] The invention provides a polyvinyl alcohol spherical microorganism carrier and a preparation method and application thereof.

[0029] The preparation method comprises the following steps:

[0030] (1) PVA (polyvinyl alcohol) and SA (sodium alginate) are added into water, stirred and mixed to dissolve evenly to form a PVS-SA mixed solution, and then cooled to room temperature for use;

[0031] Among them, the PVA model used in the experiment is 2699, which can only be dissolved at 90-100°C;

[0032] Therefore, in step (1), the following method is used to dissolve the substance uniformly:

[0033] Heat water to 90-100°C and stir at 150-300 rpm to dissolve it. Stir for 2-3 hours until no visible tiny particles are left. Then keep warm and stir for more than 6 hours to fully dissolve the PVA.

[0034] (2) dissolving boric acid and calcium chloride in water to prepare a boric acid-calcium chloride mixed solution, which is a coagulation bath solution;

[0035] (3) adding the PVA-SA mixed solution described in step (1) dropwise to the cross-coagulation bath described in step (2) under stirring conditions for coagulation and forming, and then allowing it to stand for full cross-linking to obtain PVA gel beads;

[0036] (4) taking out the PVA gel beads obtained in step (3), washing them, and then immersing them in a phosphate solution for esterification. After the esterification is completed, washing them to obtain PVA gel beads.

[0037] The specific method for testing the hydrolysis resistance of the esterified gel beads of the present invention is as follows:

[0038] Swelling rate determination: Weigh a certain amount of W0 dried gel beads, put them into a beaker of sodium bicarbonate buffer solution with a pH of 7.5, and let them stand at a constant temperature of 30°C for a certain time t. Take out the gel beads, dry them with absorbent paper and weigh them Wt. Calculate the swelling rate according to the following formula:

[0039]

[0040] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.

[0041] Example 1

[0042] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, and then take the small ball The mixture was washed twice with tap water because of the temperature difference when the PVA-SA mixture was pumped out. Solidified mixture would remain in the outlet part and the amount of mixture dropped into the cross-linking agent was different, which resulted in deviation in the diameter of the obtained carrier. White polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. Then, a phosphate solution with a concentration of 0.5 M, a pH of 6, and an esterification time of 4 hours was used. The carrier was then washed with water to finally obtain 80 ml of PVA-SA mixture made of PVA gel beads with reduced water solubility, which were stored in 400 ml of tap water for use.

[0043] Example 2

[0044] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, and then take the small ball The mixture was washed twice with tap water because of the temperature difference when the PVA-SA mixture was pumped out. Solidified mixture would remain in the outlet part and the amount of mixture dropped into the cross-linking agent was different, which resulted in deviation in the diameter of the obtained carrier. White polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. Then, a phosphate solution with a concentration of 0.5 M, a pH of 6, and an esterification time of 6 hours was used. The carrier was then washed with water to finally obtain 80 ml of PVA-SA mixture made of PVA gel beads with reduced water solubility, which were stored in 400 ml of tap water for use.

[0045] Example 3

[0046] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, and then take the small ball The mixture was washed twice with tap water because of the temperature difference when the PVA-SA mixture was pumped out. Solidified mixture would remain in the outlet part and the amount of mixture dropped into the cross-linking agent was different, which resulted in deviation in the diameter of the obtained carrier. White polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. Then, a phosphate solution with a concentration of 0.5 M, a pH of 6, and an esterification time of 8 hours was used. The carrier was then washed with water to finally obtain 80 ml of PVA-SA mixture made of PVA gel beads with reduced water solubility, which were stored in 400 ml of tap water for use.

[0047] Comparative Example 1

[0048] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, crosslink at room temperature for 24 hours, and then The balls were taken out and washed twice with tap water. Because there was a temperature difference when the PVA-SA mixture was pumped out, solidified mixture would remain at the outlet. The amount of mixture dripped into the cross-linking agent was different, resulting in deviations in the diameter of the obtained carrier. A white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. It was then washed with a phosphate solution with a concentration of 0.5 M and a pH of 6 without esterification, and then washed with water to finally obtain 80 ml of PVA-SA mixture as a carrier to reduce the water solubility of PVA gel beads, which were stored in 400 ml of tap water for use.

[0049] Comparative Example 2

[0050] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, and then take the small ball The mixture was washed twice with tap water because of the temperature difference when the PVA-SA mixture was pumped out. Solidified mixture would remain in the outlet part and the amount of mixture dropped into the cross-linking agent was different, which resulted in deviation in the diameter of the obtained carrier. White polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. Then, a phosphate solution with a concentration of 0.5 M, a pH of 6, and an esterification time of 1 hour was used. The carrier was then washed with water to finally obtain 80 ml of PVA-SA mixture made of PVA gel beads with reduced water solubility, which were stored in 400 ml of tap water for use.

[0051] Comparative Example 3

[0052] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the PVA-SA mixed solution obtained above into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, and then take the small ball The mixture was washed twice with tap water because of the temperature difference when the PVA-SA mixture was pumped out. Solidified mixture would remain in the outlet part and the amount of mixture dropped into the cross-linking agent was different, which resulted in deviation in the diameter of the obtained carrier. White polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm was obtained. Then, a phosphate solution with a concentration of 0.5 M and a pH of 6 was used for the esterification time of 2 hours. The carrier was then washed with water to finally obtain 80 ml of PVA-SA mixture made of a carrier with reduced water solubility of PVA gel beads, which were stored in 400 ml of tap water for use.

[0053] The preparation methods of Examples 2-3 and Comparative Examples 1-3 are the same as those of Example 1, except that the esterification time is changed. The swelling rate of the PVA gel beads prepared in Examples 1-3 and Comparative Examples 1-3 is tested respectively. The test results are as follows: Figure 1As shown, the swelling rate of Examples 1-3 in 20 hours is 100%-200%, and the swelling rate of Comparative Examples 1-3 in 20 hours is 200%-600%; the mass transfer efficiency of the PVA gel beads prepared in Examples 1-3 and Comparative Examples 1-3 was tested respectively, and the test results are as follows Figure 2 As shown, the mass transfer efficiency of Examples 1-3 in 20 hours is 80%-90%, and the mass transfer efficiency of Comparative Examples 1-3 in 20 hours is 10%-70%. These experimental results show that when the esterification time is greater than or equal to 4 hours, the swelling performance and mass transfer efficiency of the gel beads are better, and the gel beads can maintain a stable structure in water and are not easy to hydrolyze.

[0054] Example 4

[0055] Take 100 mL of water, add 10 g of polyvinyl alcohol (PVA) and 3 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the above-obtained PVA-SA mixed solution into 15% H2BO3 and 4% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, then take out the small ball and wash it twice with tap water, because there is a temperature difference when pumping out the PVA-SA mixed solution, There will be solidified mixed liquid remaining in the mouth part, and the amount of mixed liquid dripped into the cross-linking agent is different, which leads to deviation in the diameter of the obtained carrier, and a white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm is obtained. Then, a phosphate solution with a concentration of 0.5M, a pH of 6, and an esterification time of 4 hours is used, followed by washing with water, and finally 80 ml of PVA-SA mixed liquid is obtained. The carrier reduces the water solubility of PVA gel beads, which are stored in 400 ml of tap water for use, and then the swelling rate test and mass transfer efficiency test are carried out. Within 0 to 20 hours, the swelling rate test results are between 0% and 200%, and the mass transfer efficiency can reach a maximum of 80% to 90%.

[0056] Example 5

[0057] Take 100mL of water, add 10g of polyvinyl alcohol (PVA) and 3g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3mm to drop the above-obtained PVA-SA mixed solution into 20% H2BO3 and 5% CaCl2 by mass fraction, cross-link at room temperature for 24h, then take out the small ball and wash it twice with tap water, because there is a temperature difference when pumping out the PVA-SA mixed solution, There will be solidified mixed liquid remaining in the mouth part, and the amount of mixed liquid dripped into the cross-linking agent is different, which leads to deviation in the diameter of the obtained carrier, and a white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm is obtained. Then, a phosphate solution with a concentration of 0.5M, a pH of 6, and an esterification time of 4 hours is used, followed by washing with water, and finally 80 ml of PVA-SA mixed liquid is obtained. The carrier reduces the water solubility of PVA gel beads, which are stored in 400 ml of tap water for use, and then the swelling rate test and mass transfer efficiency test are carried out. Within 0 to 20 hours, the swelling rate test results are between 0% and 200%, and the mass transfer efficiency can reach a maximum of 80% to 90%.

[0058] Example 6

[0059] Take 100mL of water, add 11g of polyvinyl alcohol (PVA) and 2g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3mm to drop the above-obtained PVA-SA mixed solution into 10% H2BO3 and 3% CaCl2 by mass fraction, cross-link at room temperature for 24h, then take out the small ball and wash it twice with tap water, because there is a temperature difference when pumping out the PVA-SA mixed solution, There will be solidified mixed liquid remaining in the mouth part, and the amount of mixed liquid dripped into the cross-linking agent is different, which leads to deviation in the diameter of the obtained carrier, and a white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm is obtained. Then, a phosphate solution with a concentration of 0.5M, a pH of 6, and an esterification time of 4 hours is used, followed by washing with water, and finally 80 ml of PVA-SA mixed liquid is obtained. The carrier reduces the water solubility of PVA gel beads, which are stored in 400 ml of tap water for use, and then the swelling rate test and mass transfer efficiency test are carried out. Within 0 to 20 hours, the swelling rate test results are between 0% and 200%, and the mass transfer efficiency can reach a maximum of 80% to 90%.

[0060] Example 7

[0061] Take 100mL of water, add 11g of polyvinyl alcohol (PVA) and 2g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3mm to drop the above-obtained PVA-SA mixed solution into 15% H2BO3 and 4% CaCl2 by mass fraction, cross-link at room temperature for 24h, then take out the small ball and wash it twice with tap water, because there is a temperature difference when pumping out the PVA-SA mixed solution, There will be solidified mixed liquid remaining in the mouth part, and the amount of mixed liquid dripped into the cross-linking agent is different, which leads to deviation in the diameter of the obtained carrier, and a white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm is obtained. Then, a phosphate solution with a concentration of 0.5M, a pH of 6, and an esterification time of 4 hours is used, followed by washing with water, and finally 80 ml of PVA-SA mixed liquid is obtained. The carrier reduces the water solubility of PVA gel beads, which are stored in 400 ml of tap water for use, and then the swelling rate test and mass transfer efficiency test are carried out. Within 0 to 20 hours, the swelling rate test results are between 0% and 200%, and the mass transfer efficiency can reach a maximum of 80% to 90%.

[0062] Example 8

[0063] Take 100 mL of water, add 11 g of polyvinyl alcohol (PVA) and 2 g of sodium alginate (SA) to the water in turn; heat the water bath to 95°C, stir and dissolve for 2 hours until no particles are visible to the naked eye, continue stirring at 95°C for 6 hours until it is completely dissolved; finally obtain a mixed solution; let it stand for 1 hour to degas to remove the bubbles generated during the stirring process; use a peristaltic pump with a terminal nozzle diameter of 3 mm to drop the above-obtained PVA-SA mixed solution into 20% H2BO3 and 5% CaCl2 by mass fraction, cross-link at room temperature for 24 hours, then take out the small ball and wash it twice with tap water, because there is a temperature difference when pumping out the PVA-SA mixed solution, There will be solidified mixed liquid remaining in the mouth part, and the amount of mixed liquid dripped into the cross-linking agent is different, which leads to deviation in the diameter of the obtained carrier, and a white polyvinyl alcohol microbial spherical carrier with an average diameter of 3-4 mm is obtained. Then, a phosphate solution with a concentration of 0.5M, a pH of 6, and an esterification time of 4 hours is used, followed by washing with water, and finally 80 ml of PVA-SA mixed liquid is obtained. The carrier reduces the water solubility of PVA gel beads, which are stored in 400 ml of tap water for use, and then the swelling rate test and mass transfer efficiency test are carried out. Within 0 to 20 hours, the swelling rate test results are between 0% and 200%, and the mass transfer efficiency can reach a maximum of 80% to 90%.

[0064] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a polyvinyl alcohol spherical microbial carrier, characterized in that: include: Adding polyvinyl alcohol and sodium alginate into water to form a polyvinyl alcohol-sodium alginate mixed solution, wherein the mass fraction of polyvinyl alcohol is 10%-11%, and the mass fraction of sodium alginate is 2%-3%; Dissolving boric acid and calcium chloride in water to form a boric acid-calcium chloride mixed solution, wherein the mass fraction of boric acid is 10%-20%, and the mass fraction of calcium chloride is 3%-5%; The polyvinyl alcohol-sodium alginate mixed solution is added dropwise to the boric acid-calcium chloride mixed solution for full cross-linking, then washed with water, and then immersed in a phosphate solution for esterification to obtain polyvinyl alcohol gel beads.

2. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: The polyvinyl alcohol is a powdery solid with a particle size of 100 meshes.

3. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: The purity of the sodium alginate is greater than or equal to 98% by mass.

4. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: In the polyvinyl alcohol-sodium alginate mixed solution, the mass fraction of polyvinyl alcohol is 10% and the mass fraction of sodium alginate is 2%.

5. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: In the boric acid-calcium chloride mixed solution, the mass fraction of boric acid is 10%, and the mass fraction of calcium chloride is 3%.

6. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: The dropping refers to dropping the polyvinyl alcohol-sodium alginate mixed solution into the boric acid-calcium chloride mixed solution at a height of 20 cm using an instrument with a tube orifice with an inner diameter of 3 mm at the end.

7. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: The phosphate solution has a concentration of 0.5 M and a pH of 6-7.

8. The method for preparing the polyvinyl alcohol spherical microorganism carrier according to claim 1, characterized in that: The esterification time is greater than or equal to 4 hours.

9. The preparation method as claimed in claim 1 produces a polyvinyl alcohol spherical microbial carrier.

10. Use of the polyvinyl alcohol spherical microbial carrier as claimed in claim 9 in living cell immobilization technology.

Citation Information

Cited By

  • Preparation of intrinsic yellow alginate / polyvinyl alcohol composite material

    CN119798894A

  • Embedded microspheres for in-situ culture of Vibrio harveyi and culture method

    CN121538210A