Back contact battery and preparation method thereof
By forming a dense carbon doped silicon nitride mask layer during the annealing of the first semiconductor layer of the back contact battery, the problems of mask layer thickness and cost in the prior art are solved, and the corrosion resistance and conversion efficiency of the battery are improved , and simplifies the process flow.
Patent Information
- Application Number
- CN202411297182.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The existing back contact battery rear-flowing production process requires a thicker mask layer to be deposited, which increases the process flow and equipment cost. At the same time, the large thickness of the mask layer requires high laser energy, which affects the performance of the battery.
During the annealing process of the first semiconductor layer, the carbon doped silicon nitride oxide mask layer is synchronized, and the oxygen doped, nitrogen doped, and carbon doped concentration ratio is controlled to form a dense mask layer, reducing the thickness of the mask layer, and doping the phosphorus and Carbon doping improves the density and corrosion resistance of the mask layer.
A thinner mask layer is achieved to protect the first semiconductor layer, improve the corrosion resistance and conversion efficiency of the battery, and simplify the process flow, reduce equipment investment, and avoid the use of high laser energy.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a back contact battery and a preparation method thereof. Background Art
[0002] In the existing post-texturing process of back-contact cells, after depositing the first semiconductor layer on the back of the silicon wafer, it is generally necessary to deposit a first mask layer to protect the first semiconductor layer and prevent the first semiconductor layer from being corroded and damaged by the subsequent texturing solution.
[0003] However, the deposition of the first mask layer increases the process flow and equipment cost. Moreover, the existing mask layer thickness is 60nm-100nm, which requires relatively high laser energy.
[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the defect of the prior art that a thicker first mask layer needs to be deposited in the post-texturing process of a back-contact battery, which increases the process flow and equipment costs. A back-contact battery and a preparation method thereof are provided, which does not require a separate deposition of a mask layer, but rather a process in which the mask layer is formed simultaneously during the annealing of the first semiconductor layer. The required mask layer is relatively thin and the first semiconductor layer has good density, thereby ensuring that the first semiconductor layer has better corrosion resistance in the solution, improving the passivation effect, and thus improving the battery conversion efficiency. At the same time, the present invention can simplify the process flow and reduce equipment investment.
[0006] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing a back contact battery, comprising the following steps:
[0007] S1, provide double-sided polished silicon wafers;
[0008] S2, forming a first semiconductor layer on the back side of the silicon wafer; the first semiconductor layer comprises a tunneling oxide layer and an N-type doped polysilicon layer deposited in sequence, the tunneling oxide layer and the N-type doped polysilicon layer are deposited in sequence in a tubular polysilicon deposition furnace and annealed, and a carbon-nitrogen-doped silicon oxide mask layer is formed during the annealing process;
[0009] In addition, during the deposition process, the N-type doped polysilicon layer is controlled to be doped with phosphorus and carbon, and its phosphorus doping concentration and carbon doping concentration increase gradually in the direction away from the silicon wafer; the phosphorus doping concentration of the N-type doped polysilicon layer ranges from 0 to 5.5×10 20 cm -3 , the carbon doping concentration range is 5.2×10 17 cm -3 -5.4×1019 cm -3 ;
[0010] Ammonia and oxygen are introduced during the annealing to control the oxygen concentration of the carbon-nitride-doped silicon oxide mask layer to be 1×10 18 cm -3 -5×10 18 cm -3 , and the ratio of oxygen doping concentration, nitrogen doping concentration and carbon doping concentration of the carbon-nitride-doped silicon oxide mask layer is 1: (3.3-16): (1.1-10.8), and the thickness of the carbon-nitride-doped silicon oxide mask layer is 20-50nm;
[0011] S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0012] S4, then performing texturing cleaning, and then using a cleaning solution to remove the carbon-doped silicon oxide mask layer outside the second semiconductor opening region on the back side of the silicon wafer;
[0013] S5, depositing a second semiconductor layer on the back surface obtained in S4.
[0014] In some preferred embodiments of the present invention, in S2, the thickness of the N-type doped polysilicon layer is 110-160 nm.
[0015] In some preferred embodiments of the present invention, in S2, the N-type doped polysilicon layer comprises a multilayer structure and includes at least a first layer, a second layer, and a third layer, and the thickness distance between the corresponding outer edge of each layer and the outer surface of the tunneling oxide layer is d1, d2, and d3, respectively, and the thickness distance and the phosphorus doping concentration Np and the carbon doping concentration Nc of the corresponding layer satisfy:
[0016] d1≤30nm, the first layer corresponds to Np of 0-5×10 18 cm -3 , the first layer corresponds to Nc of 5.2×10 17 cm -3 -9×10 17 cm -3 ; 30nm<d2≤100nm, the second layer corresponds to Np of 3×10 19 cm -3 -9.5×10 19 cm -3 , the second layer corresponds to Nc of 1.5×10 18 cm -3 -5.4×10 18 cm -3 ; d3>100nm, the third layer corresponds to Np of 1×10 20 cm -3 -5.5×10 20 cm-3 , the third layer corresponds to Nc of 1×10 19 cm -3 -5.4×10 19 cm -3 .
[0017] In some preferred embodiments of the present invention, in S2, the deposition conditions of the N-type doped polysilicon layer include: a silane flow rate of 1000-3000sccm, a hydrogen-phosphine mixed gas flow rate of 1000-2500sccm, a methane flow rate of 30-200sccm, and a hydrogen flow rate of 7000-9000sccm; a pressure of 400-500Pa, a power supply of 5-20kW, and a time of 800-2300s.
[0018] In some preferred embodiments of the present invention, the annealing conditions include: an ammonia flow rate of 5000-15000 sccm, an oxygen flow rate of 1000-5000 sccm; an annealing temperature of 850-950° C., a pressure of 5000-50000 Pa, and a time of 30-60 min.
[0019] In some preferred embodiments of the present invention, in S2, the nitrogen doping concentration of the carbon-nitride-doped silicon oxide mask layer is 5×10 19 cm -3 -9×10 19 cm -3 .
[0020] In some preferred embodiments of the present invention, laser is used to perform the first etching of the opening in S3, and the pulse width of the laser used is less than 10 ns, and the power of the laser used is 10-50 kW.
[0021] In some preferred embodiments of the present invention, in S5, the second semiconductor layer is a stacked layer including an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer, or is a stacked layer including a tunneling oxide layer and a P-type doped polysilicon layer.
[0022] In some preferred embodiments of the present invention, in S5, the second semiconductor layer is a stacked layer comprising an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer, the thickness of the intrinsic hydrogenated amorphous silicon layer is 4-8 nm, and the thickness of the P-type doped silicon layer is 6-12 nm.
[0023] In some preferred embodiments of the present invention, the deposition temperature of the second semiconductor layer is 150-250°C.
[0024] In some preferred embodiments of the present invention, the method for preparing the back contact battery further comprises:
[0025] S6, forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer;
[0026] S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0027] S8, depositing a conductive film layer on the back surface obtained in S7;
[0028] S9, performing a third etching opening on a portion of the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0029] S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0030] In a second aspect, the present invention provides a back-contact battery, which is prepared by the method for preparing a back-contact battery described in the first aspect.
[0031] Beneficial effects:
[0032] The present invention adopts the above technical scheme, especially during the annealing process of the N-type doped polysilicon layer deposition, ammonia and oxygen are introduced. Ammonia and oxygen are decomposed into nitrogen and oxygen ions under annealing conditions, and react with the carbon-containing polysilicon film of the N-type doped polysilicon layer to form a carbon-nitrogen-doped silicon oxide film layer. This mask layer is denser due to the doping of carbon and oxygen elements, and the thickness is only about 50% of the existing process. The thickness can be reduced to 20-50nm to protect the first semiconductor layer from subsequent texturing solution corrosion. The mask layer of the present invention does not need to be deposited separately, but the process of forming the mask layer synchronously during the annealing of the first semiconductor layer is adopted. At the same time, the N-type doped polysilicon layer is doped with phosphorus and carbon, and its phosphorus doping concentration and carbon doping concentration increase in a gradient in the direction away from the silicon wafer, which can improve the passivation effect and ensure the conductive performance, and is conducive to increasing the density of the N-type doped polysilicon layer, thereby ensuring that the first semiconductor layer plays a better anti-corrosion role in the solution, improving the passivation effect, and thus improving the battery conversion efficiency; at the same time, the present invention can simplify the process flow and reduce equipment investment. Under the same conditions, if the N-type doped polysilicon layer is replaced with P-type doped polysilicon, the open circuit voltage and current density will be affected, and the battery performance will be relatively low.
[0033] Among them, the present invention also controls the ratio of oxygen doping concentration, nitrogen doping concentration and carbon doping concentration of the carbon-nitride-doped silicon oxide mask layer within an appropriate range, which is beneficial for the mask layer to be resistant to strong alkaline solutions such as texturing solution, and to control the corrosion rate of the mask layer in the cleaning solution (such as strong acid such as HF) when being removed, thereby avoiding the underlying polysilicon layer from being damaged by excessive immersion in acid solution. DETAILED DESCRIPTION
[0034] In the present invention, unless otherwise specified, directional words such as "up, down, left, right" used generally refer to the directional understanding shown in actual applications.
[0035] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0036] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0037] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0038] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.
[0039] In a first aspect, the present invention provides a method for preparing a back contact battery, comprising the following steps:
[0040] S1, provide double-sided polished silicon wafers;
[0041] S2, forming a first semiconductor layer on the back side of the silicon wafer; the first semiconductor layer comprises a tunneling oxide layer and an N-type doped polysilicon layer deposited in sequence, the tunneling oxide layer and the N-type doped polysilicon layer are deposited in sequence in a tubular polysilicon deposition furnace and annealed, and a carbon-nitrogen-doped silicon oxide mask layer is formed during the annealing process;
[0042] In addition, during the deposition process, the N-type doped polysilicon layer is controlled to be doped with phosphorus and carbon, and its phosphorus doping concentration and carbon doping concentration increase gradually in the direction away from the silicon wafer; the phosphorus doping concentration of the N-type doped polysilicon layer ranges from 0 to 5.5×10 20 cm -3 , the carbon doping concentration range is 5.2×10 17 cm -3 -5.4×10 19 cm -3 ;
[0043] Ammonia and oxygen are introduced during the annealing to control the oxygen concentration of the carbon-nitride-doped silicon oxide mask layer to be 1×10 18 cm -3 -5×10 18 cm -3 , and the ratio of oxygen doping concentration, nitrogen doping concentration and carbon doping concentration of the carbon-nitride-doped silicon oxide mask layer is 1: (3.3-16): (1.1-10.8), preferably 1: (12-16): (1.1-10.8), and the thickness of the carbon-nitride-doped silicon oxide mask layer is 20-50 nm;
[0044] S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0045] S4, then performing texturing cleaning, and then using a cleaning solution to remove the carbon-doped silicon oxide mask layer outside the second semiconductor opening region on the back side of the silicon wafer;
[0046] S5, depositing a second semiconductor layer on the back surface obtained in S4.
[0047] In some preferred embodiments of the present invention, in S2, the thickness of the N-type doped polysilicon layer is 110-160 nm. Using an appropriately thick N-type doped polysilicon layer is more conducive to taking into account the passivation effect, conductive properties and optical properties.
[0048] In some specific embodiments of the present invention, in S2, the N-type doped polysilicon layer comprises a multilayer structure and includes at least a first layer and a second layer, and the thickness distance between the corresponding outer edge of each layer and the outer surface of the tunneling oxide layer is d1 and d2 respectively, and the thickness distance and the phosphorus doping concentration Np and the carbon doping concentration Nc of the corresponding layer satisfy:
[0049] d1≤30nm, the first layer corresponds to Np of 0-5×10 18 cm -3 , it is more preferred that the first layer corresponds to Np is 0; the first layer corresponds to Nc is 5.2×10 17 cm -3 -9×10 17 cm -3 ;
[0050] 30nm<d2≤100nm, the second layer corresponds to Np of 3×10 19 cm -3 -9.5×10 19 cm -3 , the second layer corresponds to Nc of 1.5×10 18 cm -3 -5.4×10 18 cm -3 .
[0051] In some more preferred embodiments of the present invention, in S2, the N-type doped polysilicon layer comprises a multilayer structure and includes at least a first layer, a second layer, and a third layer, and the thickness distance between the corresponding outer edge of each layer and the outer surface of the tunneling oxide layer is d1, d2, and d3, respectively, and the thickness distance and the phosphorus doping concentration Np and the carbon doping concentration Nc of the corresponding layer satisfy:
[0052] d1≤30nm, the first layer corresponds to Np of 0-5×10 18 cm -3 , it is more preferred that the first layer corresponds to Np is 0; the first layer corresponds to Nc is 5.2×10 17 cm -3 -9×10 17 cm -3 ;
[0053] 30nm<d2≤100nm, the second layer corresponds to Np of 3×10 19 cm -3 -9.5×10 19 cm -3 , the second layer corresponds to Nc of 1.5×10 18 cm -3 -5.4×10 18 cm -3 ;
[0054] d3>100nm, the third layer corresponds to Np of 1×10 20 cm -3 -5.5×10 20 cm -3 , the third layer corresponds to Nc of 1×10 19 cm -3 -5.4×10 19 cm -3. It can be understood that d2 includes d1, and d3 includes d2. Exemplarily, the first layer corresponds to Np and the first layer corresponds to Nc refers to the phosphorus doping concentration Np and the carbon doping concentration Nc of the first layer, and the same applies to other layers corresponding to Np and Nc. Exemplarily, when the N-type doped polysilicon layer is divided into three layers, the thickness of the first two layers is determined and is 30nm and 70nm respectively (the corresponding thickness distances between the corresponding outer edges of the first two layers and the outer surface of the tunneling oxide layer are 30nm and 100nm respectively), and the thickness of the last layer varies with the change of the polysilicon thickness, and the doping conditions of different layers meet the above conditions.
[0055] The use of the above-mentioned N-type doped polysilicon layer whose doping concentration changes with the thickness distance is more conducive to ensuring the passivation effect of the film layer. Suitable phosphorus doping is beneficial to improving the conductivity of the polysilicon film layer and preventing the possibility of phosphorus element being precipitated during the annealing process of the film layer and causing the concentration to decrease. At the same time, suitable carbon doping is conducive to improving the density of the polysilicon film layer and improving the corrosion resistance of the polycrystalline film layer. Therefore, the corrosion resistance is improved while ensuring the passivation effect of the N-type doped polysilicon layer.
[0056] In some preferred embodiments of the present invention, in S2, the deposition conditions of the N-type doped polysilicon layer include: a flow rate of silane of 1000-3000sccm, a flow rate of a mixed gas of hydrogen and phosphine of 1000-2500sccm, a flow rate of methane of 30-200sccm, and a flow rate of hydrogen of 7000-9000sccm. The ratio of hydrogen to phosphine in the mixed gas of hydrogen and phosphine can be adjusted according to the required phosphorus doping concentration, for example, the flow rate ratio of hydrogen to phosphine can be 30-60:1.
[0057] In some preferred embodiments of the present invention, in S2, the deposition conditions of the N-type doped polysilicon layer include: a pressure of 400-500 Pa, a power of 5-20 kW, and a time of 800-2300 s.
[0058] In the present invention, the oxygen doping concentration of the N-type doped polysilicon layer can be controlled by adjusting the flow parameters of the oxygen introduced during annealing, the nitrogen doping concentration can be controlled by adjusting the flow parameters of the ammonia introduced during annealing, and the carbon doping concentration can be controlled by adjusting the flow parameters of the methane introduced during the deposition of polysilicon.
[0059] In some preferred embodiments of the present invention, the annealing conditions include: an ammonia flow rate of 5000-15000 sccm, and an oxygen flow rate of 1000-5000 sccm.
[0060] In some preferred embodiments of the present invention, the annealing conditions include: annealing temperature of 850-950° C., pressure of 5000-50000 Pa, and time of 30-60 min.
[0061] In some preferred embodiments of the present invention, in S2, the nitrogen doping concentration of the carbon-nitride-doped silicon oxide mask layer is 5×10 19 cm -3 -9×10 19 cm -3 The use of a carbon-nitride-doped silicon oxide mask layer with a suitable nitrogen doping concentration is more conducive to improving the protective effect of the mask layer.
[0062] The first etching of the opening in S3 can be done by laser or mask etching, as long as the second semiconductor opening region can be formed. The laser can be ultraviolet or green laser.
[0063] In some preferred embodiments of the present invention, laser is used to perform the first etching opening in S3, and the pulse width of the laser is less than 10ns, and the power of the laser used is 10-50kW. The present invention uses a laser power that is 30-50% lower than that of the existing process to perform the first etching opening to remove the first semiconductor layer and the thinner carbon-doped silicon oxide mask layer on its surface, while quickly removing these film layers, it virtually reduces the depreciation loss of the laser equipment and increases the service life.
[0064] In some preferred embodiments of the present invention, in S5, the second semiconductor layer is a stacked layer including an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer, or is a stacked layer including a tunneling oxide layer and a P-type doped polysilicon layer.
[0065] In some preferred embodiments of the present invention, in S5, the second semiconductor layer is a stacked layer comprising an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer. The preparation method of the present invention is combined with a combined passivation structure to further improve the overall passivation effect and current density of the battery.
[0066] Further preferably, the thickness of the intrinsic hydrogenated amorphous silicon layer is 4-8 nm, and the thickness of the P-type doped silicon layer is 6-12 nm. The P-type doped silicon layer may be a P-type doped microcrystalline silicon layer or a doped amorphous silicon layer.
[0067] The second semiconductor layer can be formed, for example, by plate-type CVD. In some preferred embodiments of the present invention, the deposition temperature of the second semiconductor layer is 150-250°C.
[0068] Preferably, in the present invention, the thickness of the tunneling oxide layer in the first semiconductor layer is 1-2 nm, and / or the thickness of the tunneling oxide layer in the second semiconductor layer is 1-2 nm. The preparation method of each tunneling oxide layer (such as a tunneling silicon oxide layer) can refer to the prior art, as long as a film layer of the target thickness is obtained, for example, it can be formed by tubular PECVD, LPCVD or PVD, preferably by deposition in a tubular polysilicon deposition furnace, and the deposition temperature is 400-500 ° C. Exemplarily, the deposition conditions of the tunneling oxide layer include: controlling the flow rate of the laughing gas to 8000-12000 sccm, the pressure to 100-200 Pa, the power of the power supply to 3-20 kW, and the time to 20-100 s.
[0069] The texturing cleaning in S4 of the present invention is used to remove the residual mask layer and the first semiconductor layer in the second semiconductor opening area, and at the same time form a velvet surface on the front side of the silicon wafer and the second semiconductor opening area; the texturing liquid and texturing conditions used can refer to the existing technology, and the texturing liquid used is a mixture of alkali (such as potassium hydroxide or sodium hydroxide), texturing additives and water, wherein the mass percentage of alkali is 1%-5%, and the mass percentage of texturing additives is 0.5%-1%. Further, the texturing conditions can include: the texturing time is 8-30min, and the texturing temperature is 75℃-85℃. The texturing additives can be obtained commercially.
[0070] The cleaning solution for removing the mask layer in S4 can refer to the prior art. The carbon-nitrogen-doped silicon oxide mask layer of the present invention has a suitably low corrosion rate in a conventional cleaning solution (such as a strong acid such as HF) when being removed, so as to avoid the underlying polysilicon layer being damaged by excessive immersion in the acid solution. Exemplarily, when it is necessary to remove the mask layer, the final cleaning conditions include: the cleaning solution used for the final cleaning is an acid solution such as HF, the mass percentage of HF in the HF acid solution is 0.5%-5%, the mass percentage of deionized water contained is 95%-99.5%, the processing temperature is 20°C-30°C, and the removal time is 60-300s.
[0071] In some preferred embodiments of the present invention, the method for preparing the back-contact cell further comprises: S6, forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer.
[0072] Further, the passivation layer can be one or a combination of an amorphous silicon passivation layer, a silicon oxide passivation layer and an aluminum oxide passivation layer. Preferably, the passivation layer is a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer, the thickness of the silicon oxide passivation layer is 1-2nm, and the thickness of the aluminum oxide passivation layer is 3-4nm.
[0073] Furthermore, the anti-reflection layer can be one or a combination of a silicon nitride layer, an aluminum oxide layer and a silicon oxide layer, preferably a combination of a silicon nitride layer and a silicon oxide layer, the thickness of the silicon nitride layer is 50-100 nm, and the thickness of the silicon oxide layer is 30-80 nm.
[0074] In some preferred embodiments of the present invention, the method for preparing the back contact battery further comprises:
[0075] S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0076] S8, depositing a conductive film layer on the back surface obtained in S7;
[0077] S9, performing a third etching opening on a portion of the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove;
[0078] S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0079] Preferably, the width of the second semiconductor opening region is 400-600 μm, the width of the first semiconductor opening region is 100-250 μm, and the width of the isolation trench is 20-100 μm.
[0080] In a second aspect, the present invention provides a back-contact battery, which is prepared by the method for preparing a back-contact battery described in the first aspect.
[0081] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0082] Example 1
[0083] A method for preparing a back contact battery, the steps are as follows:
[0084] S1, N-type single crystal silicon wafer double-sided polishing:
[0085] S2, forming a first semiconductor layer on the back of the silicon wafer and annealing to form a mask layer:
[0086] The first semiconductor layer includes a tunneling silicon oxide layer and an N-type doped polysilicon layer. The tunneling silicon oxide layer has a thickness of 1.5 nm, and the N-type doped polysilicon layer has a thickness of 150 nm.
[0087] The tunneling silicon oxide layer and the N-type doped polysilicon layer are sequentially deposited and annealed at high temperature using a tubular polysilicon deposition furnace, and the deposition temperature is 450° C. When depositing the tunneling silicon oxide layer, the flow rate of laughing gas is 10000 sccm, the pressure is 150 Pa, the power is 9.5 kW, and the time is 50 s.
[0088] When depositing the N-type doped polysilicon layer, the flow rate of silane is 2000sccm, the flow rate of the mixed gas of hydrogen carrying phosphine (flow ratio of 2% PH3 / 98% H2) is 2000sccm, the flow rate of methane is 150sccm, the flow rate of hydrogen is 8000sccm, the pressure is 400Pa, the power is 10kW, and the time is 1900s. The N-type doped polysilicon layer is deposited in three layers with gradient phosphorus and carbon doping, and the thickness distance between the corresponding outer edge of each layer and the outer surface of the tunneling oxide layer is d1, d2, and d3 respectively, and the thickness distance and the phosphorus doping concentration Np and carbon doping concentration Nc of the corresponding layer meet: d1≤30nm, the first layer corresponds to Np is 0, and the first layer corresponds to Nc is 8.7×10 17 cm -3 ; 30nm<d2≤100nm, the second layer corresponds to Np of 7.5×10 19 cm -3 , the second layer corresponds to Nc of 4×10 18 cm -3 ; d3>100nm, the third layer corresponds to Np of 3.8×10 20 cm -3 , the third layer corresponds to Nc of 2.5×10 19 cm -3 .
[0089] After deposition, high temperature annealing is performed to form a carbon-doped silicon oxide mask layer. Ammonia and oxygen are introduced into the high temperature annealing. The flow rate of ammonia is 8000sccm, the flow rate of oxygen is 3000sccm, the annealing temperature is 900℃, the pressure is 10000Pa, and the time is 40min. The thickness of the carbon-doped silicon oxide film layer is 40nm, and the oxygen concentration in the carbon-doped silicon oxide film layer is 4.5×10 18 cm -3 , the ratio of oxygen doping concentration, nitrogen doping concentration and carbon doping concentration in the carbon-nitride-doped silicon oxide film layer is 1:13.3:5.6;
[0090] S3, using laser to etch an opening on the back side of the silicon wafer for the first time to form a second semiconductor opening area;
[0091] The laser is ultraviolet laser, with a pulse width of 5ns and a laser power of 20kW. The thickness of the mask layer is reduced, and the laser power is lower than that of the existing process to avoid damaging the underlying polysilicon layer. The width of the second semiconductor opening area formed is 500μm.
[0092] S4, texturing and cleaning the opening areas on the front and back sides of the silicon wafer;
[0093] The front and back opening areas of the silicon wafer are cleaned by texturing, wherein the texturing solution is a mixture of potassium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide is 1%, and the mass percentage of the texturing additive is 0.5%. The texturing time is 10 minutes, and the texturing temperature is 80°C.
[0094] During the texturing process on the front side, the carbon-doped silicon nitride oxide mask layer on the back side of the silicon wafer is also removed by the final cleaning solution. The solution used to remove the mask layer is HF acid solution, with a HF mass percentage of 2% and the balance of deionized water. The processing temperature is 25°C and the removal time is 120s.
[0095] S5, forming a second semiconductor layer on the back side of the silicon wafer;
[0096] The second semiconductor layer is a stack of an intrinsic hydrogenated amorphous silicon layer and a P-type doped amorphous silicon layer. The second semiconductor layer is formed by plate-type CVD. The thickness of the intrinsic hydrogenated amorphous silicon layer is 7 nm, the thickness of the P-type doped amorphous silicon layer is 12 nm, and the deposition temperature of the second semiconductor layer is 210°C.
[0097] S6. Forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer:
[0098] The passivation layer is a combination of a silicon oxide passivation layer and an aluminum oxide passivation layer, the thickness of the silicon oxide passivation layer is 1.5 nm, and the thickness of the aluminum oxide passivation layer is 3 nm;
[0099] The anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer. The thickness of the silicon nitride layer is 70 nm, and the thickness of the silicon oxide layer is 80 nm.
[0100] S7. Etch an opening on the back side of the silicon wafer for the second time to form a first semiconductor opening region. The width of the first semiconductor opening region is 230 μm.
[0101] S8, depositing a transparent conductive film layer on the back side of the silicon wafer;
[0102] S9. Etch an opening on the back side of the silicon wafer for the third time to form an isolation groove; the width of the isolation groove is 90 μm.
[0103] S10, forming metal electrodes on the outer surfaces of the first semiconductor opening region and the second semiconductor opening region corresponding to the back side of the silicon wafer.
[0104] Example 2
[0105] The method of Example 1 is referred to, except that the deposition conditions are adjusted to control the N-type doped polysilicon layer to have a two-layer structure, and the two-layer structure is the same as the first two layers of the three-layer structure of the N-type doped polysilicon layer in Example 1; that is, the third layer of the three-layer structure of the N-type doped polysilicon layer is not set.
[0106] Example 3
[0107] The method of Example 1 is followed, except that the phosphine flow rate is adjusted to control the first layer of the three-layer structure of the N-type doped polysilicon layer to have Np of 5×10 18 cm -3 .
[0108] Example 4
[0109] The method of Example 1 is followed, except that the nitrogen doping concentration of the carbon-nitride-doped silicon oxide mask layer is adjusted to 5×10 19 cm -3 , so that the ratio of oxygen doping concentration to nitrogen doping concentration of the carbon-nitride-doped silicon oxide mask layer is 1:11.1. The process parameters that need to be adjusted to meet the nitrogen doping concentration adjustment of the carbon-nitride-doped silicon oxide mask layer are: reducing the ammonia flow rate during annealing by 15%.
[0110] Example 5
[0111] The method of Example 1 is followed, except that the second semiconductor layer is an intrinsic hydrogenated amorphous silicon layer (with a thickness of 4 nm) and a P-type doped amorphous silicon layer (with a thickness of 8 nm and an effective doping concentration of 5×10 19 cm -3 ) stack.
[0112] Comparative Example 1
[0113] The method of Example 1 is referred to, except that the mask layer adopts a conventional process, and the N-type doped polysilicon layer has a conventional composition. Specifically, in S2, the N-type doped polysilicon layer is controlled to be a uniformly distributed film layer and its phosphorus doping concentration is 5×10 20 cm -3 , the thickness remains unchanged. After depositing the N-type doped polysilicon layer, a non-carbon-doped silicon nitride oxide mask layer with a thickness of 50nm is deposited using PECVD technology.
[0114] Comparative Example 2
[0115] The method of Example 1 is followed, except that the N-type doped polysilicon layer is of conventional composition. Specifically, in S2, the N-type doped polysilicon layer is controlled to be a uniformly distributed film layer and its phosphorus doping concentration is 5×10 20 cm -3 , thickness remains unchanged.
[0116] Comparative Example 3
[0117] The method of Example 1 is followed, except that the carbon doping concentration of the carbon-doped silicon oxynitride mask layer is adjusted to 3.2×10 17 cm -3 , so that the ratio of oxygen doping concentration to carbon doping concentration of the carbon-doped silicon oxide nitride mask layer is 1:0.07. The process parameters that need to be adjusted to meet the carbon doping concentration adjustment of the carbon-doped silicon oxide nitride mask layer are: reducing the methane flow by 95%.
[0118] Test Case
[0119] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1. The performance indicators of each of Examples 2-5 and the comparative example were converted using Example 1 as a reference benchmark, the data of Example 1 was normalized benchmark 1, and the other examples were converted based on Example 1, such as the battery conversion efficiency of Comparative Example 1 / battery conversion efficiency of Example 1 was 0.937.
[0120] Table 1
[0121]
[0122] It can be seen from the above results that, compared with the comparative example, the embodiment scheme of the present invention does not need to deposit the mask layer separately, but the mask layer is formed simultaneously during the annealing of the first semiconductor layer, and the required mask layer thickness is thin and the first semiconductor layer has good density, thereby ensuring that the first semiconductor layer has better corrosion resistance in the solution, improving the passivation effect, and thus improving the battery conversion efficiency; at the same time, the present invention can simplify the process flow and reduce equipment investment.
[0123] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred manufacturing method of the present invention is more conducive to ensuring that the first semiconductor layer has a better corrosion resistance in the solution, improving the passivation effect, and thus improving the battery conversion efficiency.
[0124] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a back contact battery, characterized in that: The steps include: S1, provide double-sided polished silicon wafers; S2, forming a first semiconductor layer on the back side of the silicon wafer; the first semiconductor layer comprises a tunneling oxide layer and an N-type doped polysilicon layer deposited in sequence, the tunneling oxide layer and the N-type doped polysilicon layer are deposited in sequence in a tubular polysilicon deposition furnace and annealed, and a carbon-nitrogen-doped silicon oxide mask layer is formed during the annealing process; In addition, during the deposition process, the N-type doped polysilicon layer is controlled to be doped with phosphorus and carbon, and its phosphorus doping concentration and carbon doping concentration increase gradually in the direction away from the silicon wafer; the phosphorus doping concentration of the N-type doped polysilicon layer ranges from 0 to 5.5×10 20 cm -3 , the carbon doping concentration range is 5.2×10 17 cm -3 -5.4×10 19 cm -3 ; Ammonia and oxygen are introduced during the annealing to control the oxygen concentration of the carbon-nitride-doped silicon oxide mask layer to be 1×10 18 cm -3 -5×10 18 cm -3 , and the ratio of oxygen doping concentration, nitrogen doping concentration and carbon doping concentration of the carbon-nitride-doped silicon oxide mask layer is 1: (3.3-16): (1.1-10.8), and the thickness of the carbon-nitride-doped silicon oxide mask layer is 20-50nm; S3, performing a first etching opening on the back surface obtained in S2 to form a second semiconductor opening region; S4, then performing texturing cleaning, and then using a cleaning solution to clean and remove the carbon-doped silicon oxide mask layer outside the second semiconductor opening area on the back side of the silicon wafer; S5, depositing a second semiconductor layer on the back surface obtained in S4.
2. The method for preparing a back contact battery according to claim 1, characterized in that: In S2, the thickness of the N-type doped polysilicon layer is 110-160 nm.
3. The method for preparing a back contact battery according to claim 1 or 2, characterized in that: In S2, the N-type doped polysilicon layer comprises a multilayer structure and includes at least a first layer, a second layer, and a third layer. The thickness distances between the corresponding outer edge of each layer and the outer surface of the tunnel oxide layer are d1, d2, and d3, respectively, and the thickness distances and the phosphorus doping concentration Np and the carbon doping concentration Nc of the corresponding layer satisfy: d1≤30nm, the first layer corresponds to Np of 0-5×10 18 cm -3 , the first layer corresponds to Nc of 5.2×10 17 cm -3 -9×10 17 cm -3 ; 30nm<d2≤100nm, the second layer corresponds to Np of 3×10 19 cm -3 -9.5×10 19 cm -3 , the second layer corresponds to Nc of 1.5×10 18 cm -3 -5.4×10 18 cm -3 ; d3>100nm, the third layer corresponds to Np of 1×10 20 cm -3 -5.5×10 20 cm -3 , the third layer corresponds to Nc of 1×10 19 cm -3 -5.4×10 19 cm -3 .
4. The method for preparing a back contact battery according to claim 1, characterized in that: In S2, the deposition conditions of the N-type doped polysilicon layer include: a silane flow rate of 1000-3000 sccm, a hydrogen-phosphine mixed gas flow rate of 1000-2500 sccm, a methane flow rate of 30-200 sccm, and a hydrogen flow rate of 7000-9000 sccm; a pressure of 400-500 Pa, a power supply of 5-20 kW, and a time of 800-2300 s; and / or, The annealing conditions include: an ammonia flow rate of 5000-15000 sccm, an oxygen flow rate of 1000-5000 sccm; an annealing temperature of 850-950° C., a pressure of 5000-50000 Pa, and a time of 30-60 min.
5. The method for preparing a back contact battery according to claim 1, characterized in that: In S2, the nitrogen doping concentration of the carbon nitride-doped silicon oxide mask layer is 5×10 19 cm -3 -9×10 19 cm -3 .
6. The method for preparing a back contact battery according to claim 1, characterized in that: In S3, laser is used to perform the first etching of the opening, and the pulse width of the laser used is less than 10 ns, and the power of the laser used is 10-50 kW.
7. The method for preparing a back contact battery according to claim 1, characterized in that: In S5, the second semiconductor layer is a stacked layer including an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer, or a stacked layer including a tunneling oxide layer and a P-type doped polysilicon layer.
8. The method for preparing a back contact battery according to claim 7, characterized in that: In S5, the second semiconductor layer is a stacked layer including an intrinsic hydrogenated amorphous silicon layer and a P-type doped silicon layer, the thickness of the intrinsic hydrogenated amorphous silicon layer is 4-8 nm, and the thickness of the P-type doped silicon layer is 6-12 nm; and / or, The deposition temperature of the second semiconductor layer is 150-250°C.
9. The method for preparing a back contact battery according to claim 1, characterized in that: The method for preparing the back contact battery also includes: S6, forming a passivation layer and an anti-reflection layer on the front side of the silicon wafer; S7, performing a second etching opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region; S8, depositing a conductive film layer on the back surface obtained in S7; S9, performing a third etching opening on a portion of the conductive film layer located between the first semiconductor opening region and the second semiconductor opening region to form an isolation groove; S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
10. A back contact battery, characterized in that: The back contact battery is prepared by the method for preparing a back contact battery as claimed in any one of claims 1 to 9.