Fiber laser based on TiTe2 saturable absorber and preparation method thereof
By using TiTe2 saturable absorbers in fiber lasers, including TiTe2-PVA films and TiTe2-side polished optical fibers, the problems of large output pulse width and low stability of fiber lasers are solved, and high repetition rates and high output power are achieved. Effect.
Patent Information
- Application Number
- CN202410915963.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-22
AI Technical Summary
The existing fiber laser output pulse width is large, low stability, small pulse energy and poor repeatability, which cannot meet the production and application requirements of high repetition frequency harmonic mode-locked, passive Q-switched fiber laser and passive soliton mode-locked fiber laser.
TiTe2 saturable absorber is used, including TiTe2-PVA film and TiTe2-side-polished fiber, and the pump source, fiber wavelength division multiplexer, erbium-doped gain fiber, polarization-independent isolator, and polarization controller are connected through fiber fusion splicing. , output coupler and single-mode fiber to form a closed-loop cavity laser.
It achieves high repetition frequency, narrow pulse width, high output power and good working stability, and overcomes the problems of low anti-damage threshold, low modulation depth, poor stability and low nonlinear absorption coefficient of traditional nanomaterials.
Smart Images

Figure CN118825762A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of laser technology, and in particular to a fiber laser based on a TiTe2 saturable absorber and a preparation method thereof. Background Art
[0002] With the development of technology, fiber lasers can generate ultrashort pulses with high peak power, narrow pulse width and wide spectrum. In particular, high repetition rate ultrashort pulse fiber lasers have been widely used in optical frequency combs, optical communications, laser ranging, high-speed optical sampling, nonlinear optical bio-imaging and other fields.
[0003] At present, there are three main methods for obtaining high repetition rate pulses: active mode locking, ultrashort cavity mode locking, and passive harmonic mode locking. Among them, active mode locking requires a high-frequency signal generator or other additional equipment outside the resonant cavity, which increases the system cost and structural complexity; although ultrashort cavity mode locking can also obtain high repetition rate pulses, it is difficult to further increase the repetition rate due to the physical length of the cavity. In contrast, passive harmonic mode locking is considered to be one of the simpler and more effective methods for generating high repetition rate pulses. On the other hand, passive harmonic mode locking is one of the main technologies for generating ultrashort pulses in fiber lasers. This technology is to add a saturable absorber to the laser resonant cavity and use its nonlinear absorption characteristics to achieve ultrashort pulses. Therefore, the core of passive mode locking technology is to find a stable and reliable saturable absorber.
[0004] At present, most saturable absorbers are semiconductor saturable absorber mirrors, but due to the high cost, complex manufacturing process and narrow working bandwidth, the in-depth application of semiconductor saturable absorber mirrors is greatly limited. Therefore, researchers are committed to finding materials with superior performance to meet the needs of pulsed laser applications. In order to meet this demand, people have conducted extensive research on new materials such as graphene, carbon nanotubes, black phosphorus and topological insulators. However, each material has some inherent limitations. For example, graphene has relatively poor light absorption ability. The structure of carbon nanotubes scatters light to a certain extent, resulting in increased insertion loss. Black phosphorus has poor stability and is easily oxidized in the air. The lasers prepared by existing saturable absorbers have large output pulse width, low stability, small pulse energy and poor repeatability, which cannot meet the production and application of high repetition rate harmonic mode-locked fiber lasers, passive Q-switched fiber lasers and passive soliton mode-locked fiber lasers. Summary of the invention
[0005] The present application provides a fiber laser based on a TiTe2 saturable absorber and a preparation method thereof, so as to solve the problems of large output pulse width, low stability, small pulse energy and poor repeatability of the existing fiber laser.
[0006] In a first aspect, the present application provides a fiber laser based on a TiTe2 saturable absorber, wherein the fiber laser comprises a TiTe2 saturable absorber, and the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber;
[0007] The fiber laser also includes a pump source, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber, which are sequentially connected by fiber fusion splicing;
[0008] The TiTe2 saturable absorber connects the single-mode optical fiber and the optical fiber wavelength division multiplexer, and the optical fiber wavelength division multiplexer, erbium-doped gain optical fiber, optical fiber coupler, polarization-independent isolator, polarization controller, output coupler, single-mode optical fiber and TiTe2 saturable absorber form a closed-loop cavity laser;
[0009] Wherein, the fiber laser is one of an ultrafast soliton mode-locked fiber laser, a passively Q-switched fiber laser and a high repetition rate harmonic mode-locked fiber laser.
[0010] In some possible implementations, when the fiber laser is an ultrafast soliton mode-locked fiber laser, the obtained pulse width and signal-to-noise ratio are 788 fs and 70 dB, respectively.
[0011] In some possible implementations, when the fiber laser is a passively Q-switched fiber laser, the maximum output power, single pulse energy, and signal-to-noise ratio are 14.2 mW, 212.9 nJ, and 70 dB, respectively.
[0012] In some possible implementations, when the fiber laser is a high repetition rate harmonically mode-locked fiber laser, the repetition frequency of the fiber laser is 1.181 GHz, corresponding to 189th-order harmonic mode-locked operation; the signal-to-noise ratio and maximum output power of the fiber laser are 45 dB and 20 mW, respectively.
[0013] In some possible implementations, the side-polished optical fiber of the TiTe2 saturable absorber has a length of 10 to 20 mm and a depth of 50 to 60 μm.
[0014] In a second aspect, the present application provides a method for preparing a fiber laser based on a TiTe2 saturable absorber, which is used to prepare the fiber laser of the first aspect, and the preparation method comprises:
[0015] Prepare a TiTe2 saturable absorber; the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber;
[0016] The TiTe2 saturable absorber is fused into the resonant cavity of the optical fiber laser, or the TiTe2 saturable absorber is transferred to the jumper connector of the optical fiber laser.
[0017] In some possible implementations, the method for preparing the TiTe2 saturable absorber includes:
[0018] Preparation of TiTe2 nanomaterials;
[0019] preparing polyvinyl alcohol colloid;
[0020] The TiTe2 nanomaterial is mixed with polyvinyl alcohol colloid to obtain a mixed solution;
[0021] The mixed solution is dropped onto a substrate to obtain a TiTe2 saturable absorber.
[0022] In some possible implementations, the method for preparing the TiTe2 saturable absorber includes:
[0023] Preparation of TiTe2 nanomaterials;
[0024] The TiTe2 nanomaterial is mixed with polyvinyl alcohol and then subjected to ultrasonic treatment and centrifugal treatment in sequence to obtain a centrifugal solution;
[0025] Taking out the centrifuged liquid and preparing it into a TiTe2 polyvinyl alcohol dispersion;
[0026] The TiTe2 polyvinyl alcohol dispersion is dropped on the beam waist region of the side-polished optical fiber, and a continuous laser is introduced into one end of the side-polished optical fiber to obtain a saturable absorber formed by TiTe2 deposited on the side-polished optical fiber.
[0027] In some possible implementations, the preparation method of the TiTe2 nanomaterial is:
[0028] Mixing TiTe2 and isopropanol in a mass ratio of 1:1 to obtain a mixed solution;
[0029] The mixed solution is subjected to ultrasonic treatment and centrifuged to obtain TiTe2 nanomaterials.
[0030] In some possible implementations, a continuous laser is passed through one end of the side-polished optical fiber, and under the action of photophoretic force, the TiTe2 is deposited on the waist surface of the side-polished optical fiber, thereby obtaining a saturable absorber in which TiTe2 is deposited on the side-polished optical fiber; the insertion loss of the saturable absorber in the communication band is less than or equal to 3dB.
[0031] From the above content, it can be known that the present application provides a fiber laser based on a TiTe2 saturable absorber and a preparation method thereof. The fiber laser includes a TiTe2 saturable absorber, and the TiTe2 saturable absorber includes a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber; the fiber laser also includes a pump source, an optical fiber wavelength division multiplexer, an erbium-doped gain optical fiber, an optical fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler, and a single-mode optical fiber connected in sequence by optical fiber fusion; the TiTe2 saturable absorber connects the single-mode optical fiber and the optical fiber wavelength division multiplexer, and the optical fiber wavelength division multiplexer, the erbium-doped gain optical fiber, the optical fiber coupler, the polarization-independent isolator, the polarization controller, the output coupler, the single-mode optical fiber, and the TiTe2 saturable absorber form a closed-loop cavity laser; wherein the fiber laser is one of an ultrafast soliton mode-locked fiber laser, a passively Q-switched fiber laser, and a high repetition rate harmonic mode-locked fiber laser. The present application uses TiTe2-PVA film and TiTe2-side-polished optical fiber as saturable absorbers in the fiber laser, overcoming the problems of low damage threshold, low modulation depth, narrow pulse width, poor stability, low nonlinear absorption coefficient, etc. based on traditional nanomaterials as saturable absorber devices; the fiber laser based on TiTe2 saturable absorber proposed in the present application solves the problems of large output pulse width, low stability, small pulse energy and poor repeatability of existing fiber lasers. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0033] Figure 1 TEM image of the TiTe2 nanomaterial prepared in Example 1;
[0034] Figure 2 This is the Raman spectrum of the TiTe2 nanomaterial prepared in Example 1;
[0035] Figure 3 AFM of the TiTe2 nanomaterial prepared in Example 1;
[0036] Figure 4 XPS of the TiTe2 nanomaterial prepared in Example 1;
[0037] Figure 5 This is the linear absorption diagram of the TiTe2 nanomaterial prepared in Example 1;
[0038] Figure 6This is a Z-scan image of the TiTe2 nanomaterial prepared in Example 1;
[0039] Figure 7 The preparation process and physical picture of the TiTe2-PVA film prepared in Example 2;
[0040] Figure 8 This is the I scan image of the TiTe2-PVA film prepared in Example 2;
[0041] Fig. 9 The preparation process and physical picture of the TiTe2-side polished optical fiber structure prepared in Example 3;
[0042] Fig.10 This is an I scan image of the TiTe2-side polished optical fiber structure prepared in Example 3;
[0043] Fig.11 A schematic diagram of a fiber laser device based on a TiTe2 saturable absorber provided in Example 4;
[0044] Fig.12 This is a spectrum diagram of the high energy Q-switched fiber pulse laser prepared in Example 5;
[0045] Fig.13 This is a pulse sequence diagram of the high energy Q-switched fiber pulse laser output prepared in Example 5;
[0046] Fig.14 This is a single pulse profile diagram output by the high energy Q-switched fiber pulse laser prepared in Example 5;
[0047] Fig.15 The radio frequency diagram of the high energy Q-switched fiber pulse laser prepared in Example 5;
[0048] Fig.16 This is the output and input power diagram of the high energy Q-switched fiber pulse laser prepared in Example 5;
[0049] Fig.17 This is a pulse energy variation diagram of the high energy Q-switched fiber pulse laser prepared in Example 5;
[0050] Fig.18 This is the spectrum of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0051] Fig.19 This is a pulse sequence diagram of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0052] Fig. 20 This is a pulse width diagram of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0053] Fig.21 This is the radio frequency diagram of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0054] Fig. 22 This is the output and input power diagram of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0055] Fig.23 This is a spectrum stability diagram of the ultrafast soliton mode-locked fiber pulse laser prepared in Example 6;
[0056] Fig.24 This is the output spectrum of the harmonic mode-locked fiber laser prepared in Example 6;
[0057] Fig.25 This is a pulse sequence diagram of the harmonic mode-locked fiber laser output prepared in Example 6;
[0058] Fig.26 This is the output RF diagram of the harmonic mode-locked fiber laser prepared in Example 6;
[0059] Fig. 27 This is a diagram of the output pulse width of the harmonic mode-locked fiber laser prepared in Example 6.
[0060] Description of reference numerals:
[0061] 1- pump source, 2- fiber wavelength division multiplexer, 3- erbium-doped gain fiber, 4- polarization-independent optical isolator, 5- polarization controller, 6- TiTe2-PVA film saturable absorber, 7- TiTe2- side-polished fiber structure saturable absorber, 8- output coupler, 9- single-mode fiber. DETAILED DESCRIPTION
[0062] The following embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following embodiments do not represent all implementations consistent with the present application. They are only examples of systems and methods consistent with some aspects of the present application as detailed in the claims.
[0063] With the development of technology, fiber lasers can generate ultrashort pulses with high peak power, narrow pulse width and wide spectrum. In particular, high repetition rate ultrashort pulse fiber lasers have been widely used in optical frequency combs, optical communications, laser ranging, high-speed optical sampling, nonlinear optical bio-imaging and other fields.
[0064] At present, there are three main methods for obtaining high repetition rate pulses: active mode locking, ultrashort cavity mode locking, and passive harmonic mode locking. Among them, active mode locking requires a high-frequency signal generator or other additional equipment outside the resonant cavity, which increases the system cost and structural complexity; although ultrashort cavity mode locking can also obtain high repetition rate pulses, it is difficult to further increase the repetition rate due to the physical length of the cavity. In contrast, passive harmonic mode locking is considered to be one of the simpler and more effective methods for generating high repetition rate pulses. On the other hand, passive harmonic mode locking is one of the main technologies for generating ultrashort pulses in fiber lasers. This technology is to add a saturable absorber to the laser resonant cavity and use its nonlinear absorption characteristics to achieve ultrashort pulses. Therefore, the core of passive mode locking technology is to find a stable and reliable saturable absorber.
[0065] At present, most saturable absorbers are semiconductor saturable absorber mirrors, but due to the high cost, complex manufacturing process and narrow working bandwidth, the in-depth application of semiconductor saturable absorber mirrors is greatly limited. Therefore, researchers are committed to finding materials with superior performance to meet the needs of pulsed laser applications. In order to meet this demand, people have conducted extensive research on new materials such as graphene, carbon nanotubes, black phosphorus and topological insulators. However, each material has some inherent limitations. For example, graphene has relatively poor light absorption ability. The structure of carbon nanotubes scatters light to a certain extent, resulting in increased insertion loss. Black phosphorus has poor stability and is easily oxidized in the air. The lasers prepared by existing saturable absorbers have large output pulse width, low stability, small pulse energy and poor repeatability, which cannot meet the production and application of high repetition rate harmonic mode-locked fiber lasers, passive Q-switched fiber lasers and passive soliton mode-locked fiber lasers.
[0066] Transition metal dichalcogenides usually have a large light absorption coefficient, a wide working bandwidth and strong stability. Titanium antimonide (TiTe2) belongs to a class of transition metal dichalcogenides and is a typical semi-metallic material. Its valence band and conduction band have a certain overlap, resulting in its unique electrical and optical properties. TiTe2 has high carrier mobility, broadband light absorption rate, and is stable in air. These excellent optoelectronic properties make TiTe2 a new type of strong saturable absorber to produce excellent pulsed lasers.
[0067] Based on this, the present application provides a method for preparing a fiber laser, a fiber laser and its application. Using TiTe2-PVA film and TiTe2-side-polished optical fiber as saturable absorbers in a fiber laser, mode locking and Q switching can be achieved respectively, with high repetition frequency, narrow pulse width, high output power and good working stability. The present application uses TiTe2-PVA film and TiTe2-side-polished optical fiber as saturable absorbers in a fiber laser, overcoming the problems of low damage threshold, low modulation depth, narrow pulse width, poor stability and low nonlinear absorption coefficient based on traditional nanomaterials as saturable absorbers.
[0068] In a first aspect, the present application provides a fiber laser based on a TiTe2 saturable absorber, wherein the fiber laser comprises a TiTe2 saturable absorber, and the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber;
[0069] The fiber laser also includes a pump source, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber, which are sequentially connected by fiber fusion splicing;
[0070] The TiTe2 saturable absorber connects the single-mode optical fiber and the optical fiber wavelength division multiplexer, and the optical fiber wavelength division multiplexer, erbium-doped gain optical fiber, optical fiber coupler, polarization-independent isolator, polarization controller, output coupler, single-mode optical fiber and TiTe2 saturable absorber form a closed-loop cavity laser;
[0071] Wherein, the fiber laser is one of an ultrafast soliton mode-locked fiber laser, a passively Q-switched fiber laser and a high repetition rate harmonic mode-locked fiber laser.
[0072] The pump source provides the fiber laser with a basic light source for exciting the laser. The wavelength division multiplexer is used to integrate two wavelengths of light into one optical fiber, that is, to integrate the pump light source and the excited laser into the same optical fiber. The function of the gain fiber is to excite the material in the gain fiber through the light emitted by the pump source to reverse the number of particles required to generate the laser in the gain fiber. The polarization-independent isolator is used to control the single-phase output of light. The polarization controller is used to control the polarization state of the laser in the resonant cavity. The optical coupler is used to observe the quality of the laser output. 90% of the light continues to circulate in the ring cavity, and 10% of the laser light is output from the ring cavity.
[0073] In some embodiments, when the fiber laser is an ultrafast soliton mode-locked fiber laser, the obtained pulse width and signal-to-noise ratio are 788 fs and 70 dB, respectively.
[0074] In some embodiments, when the fiber laser is a passively Q-switched fiber laser, the maximum output power, single pulse energy and signal-to-noise ratio are 14.2 mW, 212.9 nJ and 70 dB, respectively.
[0075] In some embodiments, when the fiber laser is a high repetition rate harmonically mode-locked fiber laser, the repetition frequency of the fiber laser is 1.181 GHz, corresponding to 189th order harmonic mode-locked operation; the signal-to-noise ratio and maximum output power of the fiber laser are 45 dB and 20 mW, respectively.
[0076] In some embodiments, the side-polished optical fiber of the TiTe2 saturable absorber has a length of 10 to 20 mm and a depth of 50 to 60 μm.
[0077] In a second aspect, the present application provides a method for preparing a fiber laser based on a TiTe2 saturable absorber, the preparation method comprising:
[0078] S1: preparing a TiTe2 saturable absorber; the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber.
[0079] TiTe2 has high carrier mobility, broadband light absorption rate, and is stable in air. TiTe2-PVA film and / or TiTe2-side-polished optical fiber as saturable absorbers have low cost, convenient and simple production process, good environmental stability, large nonlinear absorption coefficient and modulation depth, high damage resistance threshold and low saturation power density.
[0080] TiTe2-side-polished optical fiber was used as a saturable absorber to achieve ultrafast soliton mode-locking operation for the first time, indicating its great potential in the fields of nonlinear optics and ultrafast photonics.
[0081] TiTe2-side-polished optical fiber was used as a saturable absorber to achieve high repetition rate harmonic mode-locked operation (GHz) for the first time, indicating its great potential in high repetition rate mode-locked lasers.
[0082] TiTe2-PVA film as a saturable absorber achieved high-energy Q-switching operation for the first time, indicating its great potential in the field of high-energy pulsed fiber lasers.
[0083] S2: welding the TiTe2 saturable absorber into the resonant cavity of the optical fiber laser, or transferring the TiTe2 saturable absorber to the jumper connector of the optical fiber laser.
[0084] Based on the difference of saturable absorbers, the steps of preparing the fiber laser are also different. When the saturable absorber is a TiTe2-PVA film, the TiTe2-PVA film is cut into a plurality of connecting blocks, and the connecting blocks are transferred to the fiber laser jumper connector.
[0085] When the TiTe2 saturable absorber is a TiTe2-PVA film, the preparation method of the saturable absorber is:
[0086] S11: Preparation of TiTe2 nanomaterials;
[0087] TiTe2 and isopropanol in a mass ratio of 1:1 are mixed to obtain a mixed solution; isopropanol (IPA) is a solvent suitable for the exfoliation of two-dimensional materials, and isopropanol is added for rapid exfoliation.
[0088] The mixed solution is subjected to ultrasonic treatment and centrifuged to obtain TiTe2 nanomaterials.
[0089] S12: preparing polyvinyl alcohol colloid;
[0090] The polyvinyl alcohol is mixed with deionized water, heated to 70-90° C., and stirred for 5-12 hours to obtain polyvinyl alcohol colloid.
[0091] S13: mixing the TiTe2 nanomaterial with polyvinyl alcohol colloid to obtain a mixed solution;
[0092] S14: Dropping the mixed solution onto a substrate to obtain a TiTe2-PVA film.
[0093] The TiTe2 nanomaterial is mixed with polyvinyl alcohol colloid, dropped on a glass substrate, and dried to obtain a uniform TiTe2-PVA film.
[0094] By wrapping the TiTe2 nanomaterial in polyvinyl alcohol (PVA) through the above method, a saturable absorber colloidal film is prepared, which avoids the oxidation of the material, can be stably stored for a long time, and ensures stable properties.
[0095] When the TiTe2 saturable absorber is a TiTe2-side polished optical fiber, the preparation method of the saturable absorber is:
[0096] S11: Preparation of TiTe2 nanomaterials;
[0097] S12': mixing the TiTe2 nanomaterial with polyvinyl alcohol and sequentially subjecting the mixture to ultrasonic treatment and centrifugation to obtain a centrifuge solution;
[0098] S13': taking out the centrifuged liquid and preparing it into a TiTe2 polyvinyl alcohol dispersion;
[0099] S14': drop the TiTe2 polyvinyl alcohol dispersion on the beam waist region of the side-polished optical fiber, and pass a continuous laser through one end of the side-polished optical fiber to obtain a saturable absorber formed by TiTe2 deposited on the side-polished optical fiber.
[0100] A laser with a wavelength of 976nm and a power of 100mW is coupled to a side-polished optical fiber. A continuous laser is passed through one end of the side-polished optical fiber. Under the action of photophoretic force, the TiTe2 is deposited on the waist surface of the side-polished optical fiber to obtain a saturable absorber in which TiTe2 is deposited on the side-polished optical fiber; the insertion loss of the saturable absorber in the communication band is less than or equal to 3dB.
[0101] TiTe2 nanosheets are deposited on the side-polished optical fiber DSF by the above method, and the evanescent field is used to achieve a strong interaction between light and matter, and has good heat dissipation, so that the saturable absorber has a higher damage threshold.
[0102] In some embodiments, the length of the side-polished optical fiber is 10-20 mm, and the depth of the side-polished optical fiber is 50-60 μm.
[0103] The following is a detailed explanation with reference to specific cases.
[0104] In the following examples, TEM was measured by a transmission electron microscope (JEM-2200FS); Raman spectrum was measured by a Renishaw 2000 Raman spectrometer; XPS was measured by an EscaLab 250Xi model X-ray photoelectron spectrometer; AFM was measured by a Bruker Dimension Icon atomic force microscope; and linear absorption was measured by a Lambda 1050+.
[0105] Example 1
[0106] Preparation of TiTe2 nanomaterials:
[0107] 10 mg of TiTe2 powder sample was added to 10 mL of isopropyl alcohol (IPA), and the mixture was placed in an ultrasonic machine with a power of 300 W for exfoliation. The bubbles generated by the ultrasound broke the van der Waals force between the TiTe2 layers, forming a single layer or a few layers of TiTe2 nanosheets; after the mixture was ultrasonicated for 8 hours without interruption, TiTe2 nanomaterials (TiTe2 nanosheets) were obtained. The nonlinear optical absorption test of TiTe2 nanosheets was performed using a Z scanning device, and the results are as follows Figures 1 to 6 As shown, the results show that TiTe2 nanosheets have excellent wide-band saturable absorption characteristics.
[0108] Example 2
[0109] Preparation of TiTe2 saturable absorber (TiTe2-PVA film):
[0110] Pour 5 g of polyvinyl alcohol solid powder into 100 ml of deionized water, heat to 70 degrees Celsius, and stir for 12 hours to prepare PVA colloid.
[0111] 5 mL of the TiTe2 nanosheets prepared in Example 1 was completely mixed with 10 mL of PVA colloid and then dropped onto a clean glass substrate. After natural drying, a uniform TiTe2-PVA film was obtained. Figure 7 , Figure 8 As shown in FIG. 1 , the I scan curve of the TiTe2-PVA film at 1550 nm reflects the modulation depth, saturated power density and unsaturated loss. The TiTe2 saturable absorber prepared in this embodiment has excellent mode-locking stability and strong light absorption and light response in the near-infrared band. The device has a high damage threshold, fast recovery time, large modulation depth, strong stability and good heat dissipation.
[0112] Example 3
[0113] Preparation of TiTe2 saturable absorber (TiTe2-side polished optical fiber):
[0114] In this embodiment, a side-polished optical fiber DSF with a side polishing length of 17 mm and a side polishing depth of about 53 μm is used to deposit TiTe2 nanosheets.
[0115] The TiTe2 nanosheets prepared in Example 1 are mixed with isopropanol to obtain a suspension; then the TiTe2 nanosheets suspended in the isopropanol IPA solution are slowly dripped onto the surface of DSF. As the TiTe2 nanosheets are gradually deposited on the side-polished optical fiber DSF, changes in the output power can be observed. During the deposition process, the output power gradually decreases. The TiTe2 nanosheets are fully deposited on the side-polished optical fiber DSF, that is, when the output power reaches a stable state; the schematic diagram and actual picture of the TiTe2-side-polished optical fiber structure are shown in Fig. 9 As shown. Fig.10 The I scan curve of the TiTe2-side polished fiber structure at 1550nm reflects the modulation depth, saturated power density and unsaturated loss.
[0116] The TiTe2 saturable absorber prepared in this embodiment has excellent mode-locking stability and strong light absorption and light response in the near-infrared band. The device has a high damage threshold, fast recovery time, large modulation depth, strong stability and good heat dissipation.
[0117] Example 4
[0118] This embodiment provides a fiber laser including a TiTe2 saturable absorber, the fiber laser including a TiTe2 saturable absorber, a pump source, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler, and a single-mode fiber connected in sequence by fiber fusion splicing; the saturable absorber connects the single-mode fiber and the fiber wavelength division multiplexer, and the fiber wavelength division multiplexer, the gain fiber, the fiber coupler, the fiber isolator, the polarization controller, the output coupler, the single-mode fiber, and the saturable absorber form a closed-loop cavity laser. The TiTe2 saturable absorber is prepared in Example 2 and / or Example 3.
[0119] like Fig.11 As shown, the pump source 1 provides the basic light source for exciting the laser for the fiber laser, the wavelength division multiplexer 2 is used to integrate the two wavelengths of light of 980 / 1550nm into one optical fiber, the erbium-doped gain fiber 3 is used to generate the population inversion required for laser gain, the polarization-independent isolator 4 is used to control the unidirectional transmission of light, the polarization controller 5 is used to control the polarization state of the light in the cavity, the TiTe2-side-polished fiber structure and the TiTe2-PVA film are used as saturated absorbers 6, 7 for nonlinear absorption and induced mode-locking operation, and the output coupler 8 is used to observe the output laser quality.
[0120] Example 5
[0121] Preparation of high energy Q-switched fiber pulse laser using TiTe2-PVA film:
[0122] The TiTe2-PVA film prepared in Example 2 was cut and placed on a fiber laser jumper connector to prepare a high-energy Q-switched fiber pulse laser.
[0123] The passively Q-switched fiber laser includes a TiTe2 saturable absorber, a pump source connected in sequence by fiber fusion splicing, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber; the internal connection relationship of the fiber laser is the same as that in Example 4 and will not be repeated here.
[0124] The fiber laser was tested for performance, and the test results were displayed by an oscilloscope and a spectrometer. Figures 12 to 17 As shown. Fig.12 The output spectrum of the fiber laser shows that the pulse center is 1562.8nm and the spectrum presents a typical Gaussian shape. Fig.13 This is the pulse sequence diagram of the fiber laser. It can be seen that the pulse interval is 15μs, corresponding to a repetition frequency of 66.67KHz. Fig.14 The single pulse profile of the output pulse is shown, with a pulse width of only 1.6μs. Fig.15 This is the RF diagram of the Q-switched fiber laser. It can be seen that the signal-to-noise ratio is as high as 65dB, indicating that the Q-switched fiber laser has high stability. Fig.16 The relationship between the output power and input power of the Q-switched laser is shown, with a conversion efficiency of 2.5%, a maximum pump power of 568mW, and an output power of 14.2mW, proving that the Q-switched laser has a high damage resistance threshold. Fig.17 The variation of output pulse energy with pump power is shown. When the pump power is 568mW, the maximum single pulse energy is as high as 212.9nJ, which is much higher than that of lasers of the same category.
[0125] Example 6
[0126] Preparation of ultrafast soliton mode-locked fiber pulse laser or harmonic mode-locked fiber laser using TiTe2-side polished fiber:
[0127] The prepared TiTe2-side-polished optical fiber structure is integrated into the laser cavity through a fusion splicer to prepare an ultrafast soliton mode-locked fiber pulse laser or a harmonic mode-locked fiber laser.
[0128] The high repetition rate harmonically mode-locked fiber laser includes a TiTe2 saturable absorber, a pump source connected in sequence by fiber fusion splicing, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber; the internal connection relationship of the fiber laser is the same as that in Example 4 and will not be repeated here.
[0129] The ultrafast soliton mode-locked fiber laser includes a TiTe2 saturable absorber, a pump source connected in sequence by fiber fusion splicing, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber; the internal connection relationship of the fiber laser is the same as that in Example 4 and will not be repeated here.
[0130] The performance of the fiber laser is tested and the test results are displayed by an oscilloscope and a spectrometer. Figure 18-Figure 23 shown. Fig.18 The output spectrum of the fiber laser shows that the pulse center is 1560.8nm and the 3dB bandwidth is 3.4nm. Fig.19 This is the output pulse sequence diagram of the fiber laser. It can be seen that the pulse interval is 160ns, corresponding to the fundamental frequency of 6.25MHz. Fig. 20 The autocorrelation curve is shown, and the pulse width is only 788fs. Fig.21 This is the RF diagram of the harmonic mode-locked fiber laser. It can be seen that the signal-to-noise ratio is as high as 70dB, indicating that the mode-locked fiber laser has high stability. Fig. 22The relationship between the output power and input power of the mode-locked laser is shown, with a conversion efficiency of 2.0%, a maximum pump power of 378mW, and an output power of 7.56mW, proving that the mode-locked laser has a high damage resistance threshold. Fig.23 The long-term operation stability diagram of the mode-locked laser is shown. Within 3 hours of continuous operation, the spectrum did not undergo any deformation, proving its excellent long-term operation stability.
[0131] In addition, after the pump power increased by more than 378mW, stable harmonic mode-locking can be achieved by properly adjusting the polarization controller and increasing the pump power. At the maximum pump power of 800mW, a repetition frequency of up to 1.181GHz corresponding to 189th order harmonic mode-locking operation was finally achieved, and the corresponding maximum output power was up to 20mW. Fig.24 The output spectrum is shown in Figure 1, with a central wavelength of 1559nm and a 3dB bandwidth of 0.9nm. The output pulse sequence is as follows: Fig.25 As shown, it can be seen that the peak intensity of each pulse is similar and relatively stable, and the time interval between each pulse is 0.84ns, corresponding to a repetition frequency of 1.181GHz. Fig.26 The corresponding RF spectrum is shown, and an obvious peak can be observed at 1.181GHz, further proving that its repetition frequency is 1.181GHz, and its signal-to-noise ratio is 45dB, indicating that it has good stability. Finally, its corresponding output pulse width is measured, as shown in Fig. 27 As shown, its pulse width is only 1.9ps.
[0132] Example 7
[0133] This embodiment provides an ultrafast soliton mode-locked fiber laser based on a TiTe2 saturable absorber, wherein the TiTe2 saturable absorber is prepared in Example 2 and / or Example 3. The internal structure and connection relationship of the fiber laser are the same as those of Example 4 and are not described here. For the mode-locked operation, the pulse width and signal-to-noise ratio obtained are 788fs and 70dB, respectively. When the pump power is 378mW, the output power of the mode-locked laser is as high as 7.56mW, and the corresponding peak power is as high as 1535W.
[0134] Example 8
[0135] This embodiment provides a passive Q-switched fiber laser based on a TiTe2 saturable absorber, wherein the TiTe2 saturable absorber is prepared in Example 2 and / or Example 3. The internal structure and connection relationship of the fiber laser are the same as those in Example 4 and are not described here. For Q-switched pulses, the maximum output power and single pulse energy are up to 14.2 mW and 212.9 nJ respectively; the Q-switched laser has good stability and a signal-to-noise ratio of 70 dB.
[0136] Example 9
[0137] This embodiment provides a high repetition rate harmonic mode-locked fiber laser based on a TiTe2 saturable absorber, wherein the TiTe2 saturable absorber is prepared in Example 2 and / or Example 3. The internal structure and connection relationship of the fiber laser are the same as those in Example 4, and are not described here. The repetition frequency of the harmonic mode-locked laser is as high as 1.181 GHz, corresponding to the 189th order harmonic mode-locked operation; the signal-to-noise ratio of the harmonic mode-locked is 45 dB, and it has good stability; the maximum output power of the harmonic mode-locked is as high as 20 mW; the output pulse width of the harmonic mode-locked is only 1.9 ps.
[0138] As can be seen from the above embodiments, the present application provides a fiber laser based on a TiTe2 saturable absorber and a preparation method thereof. The fiber laser includes a TiTe2 saturable absorber, and the TiTe2 saturable absorber includes a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber; the fiber laser also includes a pump source, an optical fiber wavelength division multiplexer, an erbium-doped gain optical fiber, an optical fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler, and a single-mode optical fiber connected in sequence by optical fiber fusion; the TiTe2 saturable absorber connects the single-mode optical fiber and the optical fiber wavelength division multiplexer, and the optical fiber wavelength division multiplexer, the erbium-doped gain optical fiber, the optical fiber coupler, the polarization-independent isolator, the polarization controller, the output coupler, the single-mode optical fiber, and the TiTe2 saturable absorber form a closed-loop cavity laser; wherein the fiber laser is one of an ultrafast soliton mode-locked fiber laser, a passively Q-switched fiber laser, and a high repetition rate harmonic mode-locked fiber laser. This application uses TiTe2-PVA film and TiTe2-side-polished optical fiber as saturable absorbers in fiber lasers, overcoming the problems of low damage threshold, low modulation depth, narrow pulse width, poor stability, and low nonlinear absorption coefficient based on traditional nanomaterials as saturable absorber devices.
[0139] Similar parts between the embodiments provided in this application can be referenced to each other. The specific implementation methods provided above are only a few examples under the general concept of this application and do not constitute a limitation on the protection scope of this application. For those skilled in the art, any other implementation methods expanded based on the scheme of this application without creative work belong to the protection scope of this application.
Claims
1. A fiber laser based on TiTe2 saturable absorber, characterized in that: The fiber laser comprises a TiTe2 saturable absorber, and the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber; The fiber laser also includes a pump source, a fiber wavelength division multiplexer, an erbium-doped gain fiber, a fiber coupler, a polarization-independent isolator, a polarization controller, an output coupler and a single-mode fiber, which are sequentially connected by fiber fusion splicing; The TiTe2 saturable absorber connects the single-mode optical fiber and the optical fiber wavelength division multiplexer, and the optical fiber wavelength division multiplexer, erbium-doped gain optical fiber, optical fiber coupler, polarization-independent isolator, polarization controller, output coupler, single-mode optical fiber and TiTe2 saturable absorber form a closed-loop cavity laser; Wherein, the fiber laser is one of an ultrafast soliton mode-locked fiber laser, a passively Q-switched fiber laser and a high repetition rate harmonic mode-locked fiber laser.
2. The fiber laser according to claim 1, characterized in that: When the fiber laser is an ultrafast soliton mode-locked fiber laser, the obtained pulse width and signal-to-noise ratio are 788 fs and 70 dB, respectively.
3. The fiber laser according to claim 1, characterized in that: When the fiber laser is a passively Q-switched fiber laser, the maximum output power, single pulse energy and signal-to-noise ratio are 14.2 mW, 212.9 nJ and 70 dB, respectively.
4. The fiber laser according to claim 1, characterized in that: When the fiber laser is a high repetition rate harmonic mode-locked fiber laser, the repetition frequency of the fiber laser is 1.181 GHz, corresponding to 189th order harmonic mode-locked operation; the signal-to-noise ratio and maximum output power of the fiber laser are 45 dB and 20 mW, respectively.
5. The fiber laser according to claim 1, characterized in that: The side-polished optical fiber length of the TiTe2 saturable absorber is 10-20 mm, and the side-polished optical fiber depth is 50-60 μm.
6. A method for preparing a fiber laser based on a TiTe2 saturable absorber, characterized in that: Used to prepare the optical fiber laser according to any one of claims 1 to 5, the preparation method comprising: Prepare a TiTe2 saturable absorber; the TiTe2 saturable absorber comprises a TiTe2-PVA film and / or a TiTe2-side-polished optical fiber; The TiTe2 saturable absorber is fused into the resonant cavity of the optical fiber laser, or the TiTe2 saturable absorber is transferred to the jumper connector of the optical fiber laser.
7. The preparation method according to claim 6, characterized in that: The preparation method of the TiTe2 saturable absorber comprises: Preparation of TiTe2 nanomaterials; preparing polyvinyl alcohol colloid; The TiTe2 nanomaterial is mixed with polyvinyl alcohol colloid to obtain a mixed solution; The mixed solution is dropped onto a substrate to obtain a TiTe2 saturable absorber.
8. The preparation method according to claim 6, characterized in that: The preparation method of the TiTe2 saturable absorber comprises: Preparation of TiTe2 nanomaterials; The TiTe2 nanomaterial is mixed with polyvinyl alcohol and then subjected to ultrasonic treatment and centrifugal treatment in sequence to obtain a centrifugal solution; Taking out the centrifuged liquid and preparing it into a TiTe2 polyvinyl alcohol dispersion; The TiTe2 polyvinyl alcohol dispersion is dropped on the beam waist region of the side-polished optical fiber, and a continuous laser is introduced into one end of the side-polished optical fiber to obtain a saturable absorber formed by TiTe2 deposited on the side-polished optical fiber.
9. The preparation method according to claim 7 or 8, characterized in that: The preparation method of the TiTe2 nanomaterial is: Mixing TiTe2 and isopropanol in a mass ratio of 1:1 to obtain a mixed solution; The mixed solution is subjected to ultrasonic treatment and centrifuged to obtain TiTe2 nanomaterials.
10. The preparation method according to claim 8, characterized in that: A continuous laser is passed through one end of the side-polished optical fiber. Under the action of photophoretic force, the TiTe2 is deposited on the waist surface of the side-polished optical fiber to obtain a saturable absorber with TiTe2 deposited on the side-polished optical fiber; the insertion loss of the saturable absorber in the communication band is less than or equal to 3dB.