Perovskite layer, preparation method thereof and photovoltaic device
By adding succinamide to the lead iodide precursor solution to form a porous structure of lead iodide layer, the problem of difficulty in penetrating ammonium salts in the traditional process is solved, and the performance and efficiency of perovskite photovoltaic devices are improved.
Patent Information
- Application Number
- CN202311423808.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-27
- Publication Date
- 2024-10-22
AI Technical Summary
The step-by-step deposition process of the traditional two-step method to prepare the perovskite layer results in a dense lead iodide layer that makes it difficult for ammonium salts to penetrate, reducing the crystallinity of the perovskite and photovoltaic device performance.
By introducing succinamide into the lead iodide precursor solution, N-H...I hydrogen bonds are formed, the nucleation energy barrier is reduced, a porous structure of lead iodide layer is formed, and the omnidirectional diffusion and spatial confinement effect of the ammonium salt are promoted to achieve calcium Complete conversion of titanium ore.
The photoelectric conversion efficiency of perovskite photovoltaic devices is improved, and the device efficiency of perovskite or crystalline silicon stacked solar cells is improved.
Smart Images

Figure CN118829326A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic devices, and in particular to a perovskite layer and a preparation method thereof, and a photovoltaic device. Background Art
[0002] Currently, as a new type of solar cell, perovskite solar cells have the advantages of low cost, low environmental pollution, high photoelectric conversion efficiency, and the ability to prepare stacked solar cells. They have become the photovoltaic technology with the most promising commercial applications. At present, the most commonly used wide-bandgap perovskite layer preparation processes in the laboratory are divided into one-step and two-step processes. The two-step process first deposits a lead iodide layer and then deposits an ammonium salt layer to obtain a perovskite film, avoiding the use of an anti-solvent. However, due to the two-step deposition process, the dense lead iodide layer makes it difficult for ammonium salts to penetrate, often resulting in incomplete reactions between the two, reducing the crystallinity of the perovskite and seriously affecting the performance of the battery. Summary of the invention
[0003] In view of this, the present application provides a perovskite layer, a preparation method thereof, and a photovoltaic device. The lead iodide layer obtained in the preparation process of the preparation method has a porous structure, which is conducive to the downward penetration of ammonium salt during the preparation process, thereby preparing a perovskite layer and a photovoltaic device with good performance.
[0004] In a first aspect, the present application provides a method for preparing a perovskite layer, the preparation method comprising: S1, coating a lead iodide precursor solution on a surface of a substrate, and performing a first annealing treatment to prepare a lead iodide layer; S2, coating an ammonium salt solution on the lead iodide layer, and performing a second annealing treatment to obtain the perovskite layer; Wherein, the lead iodide precursor solution comprises succinamide, lead salt and solvent.
[0005] Optionally, the concentration of succinamide in the lead iodide precursor solution is 0.2-1.2 mg / mL.
[0006] Optionally, the lead salt includes one or more of PbBr2, PbI2 and PbCl2; and the solvent includes one or more of DMF, DMSO, tBP and NMP.
[0007] Optionally, the lead iodide layer has a porous structure with an average pore size of 75-85 nm.
[0008] Optionally, the ammonium salt solution includes one or more of formamidine iodide, methylammonium chloride, methylammonium iodide and methylammonium bromide.
[0009] Optionally, in step S1, the coating is spin coating, the rotation speed of the spin coating is 2000-3000 rpm, the time is 20-50 s, the acceleration is 1000-1500 rpm / s, and the temperature of the first annealing treatment is 60-80° C., and the time is 0.5-3 min.
[0010] Optionally, in step S2, the coating is spin coating, the rotation speed of the spin coating is 2500-3000 rpm, the time is 20-50 s, the acceleration is 1000-1500 rpm / s, and the temperature of the second annealing treatment is 140-160° C., and the time is 10-20 min.
[0011] In a second aspect, the present application provides a perovskite layer, which is prepared by the preparation method of the perovskite layer provided in the first aspect of the present application.
[0012] Optionally, the perovskite layer is FA x MA 1-x PbX3, wherein 0≤x≤1, and X is one or more of the halogen elements Cl, Br and I; and the thickness of the perovskite layer is 400-600nm.
[0013] Optionally, the average particle size of the perovskite grains in the perovskite layer is 900-1100 nm.
[0014] In a third aspect, the present application provides a photovoltaic device, comprising the perovskite layer provided in the second aspect of the present application.
[0015] Through the above technical solution, the present application introduces succinamide into the lead iodide precursor solution to form NH···I hydrogen bonds, which can reduce the nucleation barrier and then form a porous lead iodide layer, so that subsequent ammonium salts can penetrate more fully. Different from the traditional layer-by-layer penetration of ammonium salts, the ammonium salt solution can achieve omnidirectional diffusion and spatial confinement effects through a porous ordered array structure, effectively promoting the complete conversion of perovskite and improving the photoelectric conversion efficiency of perovskite photovoltaic devices containing the perovskite layer.
[0016] Other features and advantages of the present application will be described in detail in the subsequent detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0018] Figure 1It is a schematic diagram of the structure of a perovskite solar cell provided in an embodiment of the present application.
[0019] Figure 2 It is a flow chart of a method for preparing a perovskite solar cell provided in an embodiment of the present application.
[0020] Figure 3 This is the technical solution for preparing the perovskite layer provided in the embodiments of the present application.
[0021] Figure 4 It is an electron microscope image of the lead iodide layer in Example 3.
[0022] Figure 5 This is an electron microscope image of the lead iodide layer in Comparative Example 1.
[0023] Figure 6 This is an electron microscope image of the perovskite grains in Example 3.
[0024] Figure 7 This is an electron microscope image of the perovskite grains in Comparative Example 1.
[0025] Explanation of the reference numerals: 1 - first electrode layer, 2 - hole transport layer, 3 - perovskite layer, 4 - electron transport layer, 5 - hole blocking layer, 6 - metal electrode. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0027] The present application provides a method for preparing a perovskite layer, which is prepared by a two-step method, and the preparation method comprises: S1, applying a lead iodide precursor solution to the surface of a substrate, and performing a first annealing treatment to prepare a lead iodide layer; S2, applying an ammonium salt solution on the lead iodide layer, and performing a second annealing treatment to obtain the perovskite layer; wherein the preparation method further comprises preparing the lead iodide precursor solution, and the lead iodide precursor solution comprises succinamide, a lead salt, and a solvent. Succinamide and the lead salt are dissolved in a solvent, and heated to fully dissolve them, thereby preparing a lead iodide precursor solution.
[0028] In one embodiment of the present application, the concentration of the succinamide in the lead iodide precursor solution is 0.2-1.2mg / mL. Specifically, the concentration of succinamide in the lead iodide precursor solution can be, but is not limited to, 0.20mg / mL, 0.25mg / mL, 0.50mg / mL, 0.75mg / mL, 1.00mg / mL or 1.2mg / mL. In order to further enhance the influence of succinamide on the formation of a porous structure of the lead iodide layer, the concentration of succinamide in the lead iodide precursor solution is preferably 0.25-1.00mg / mL. In one embodiment of the present application, the concentration of succinamide in the lead iodide precursor solution is 0.15mg / mL, 0.25mg / mL, 0.50mg / mL, 0.75mg / mL, 1.00mg / mL or 1.40mg / mL.
[0029] In one embodiment of the present application, the lead salt in the lead iodide precursor solution includes one or more of PbBr2, PbI2 and PbCl2. Specifically, the lead salt in the lead iodide precursor solution can use PbBr2, PbI2 or PbCl2 alone; or use PbBr2 and PbI2, PbBr2 and PbCl2, PbBr2 and PbCl2; or use PbBr2, PbI2 and PbCl2 at the same time. In one embodiment of the present application, the lead salt in the lead iodide precursor solution includes PbBr2 and PbI2, wherein PbBr2 can be used to adjust the band gap, and the higher the proportion of Br element, the larger the band gap.
[0030] In one embodiment of the present application, the solvent in the lead iodide precursor solution includes one or more of DMF, DMSO, tBP and NMP. Specifically, the above solvents can be used alone or in combination. In one embodiment of the present application, the solvent in the lead iodide precursor solution can be a mixed solution of DMF and DMSO, and the volume ratio can be (4-19): 1. In one embodiment of the present application, the volume ratio of DMF to DMSO is 9: 1. DMF and DMSO are used together to fully dissolve lead salts.
[0031] In one embodiment of the present application, the ammonium salt solution includes one or more of formamidine iodide, methylammonium chloride, methylammonium iodide and methylammonium bromide. In one example of the present application, the ammonium salt solution includes formamidine iodide, methylammonium chloride and methylammonium bromide.
[0032] In step S1, the coating is spin coating, the rotation speed of the spin coating is 2000-3000rpm, the time is 20-50s, the acceleration is 1000-1500rpm / s, and the temperature of the first annealing treatment is 60-80°C, and the time is 0.5-3min. This process is to accelerate from a standstill at the acceleration of 1000-1500rpm / s until the rotation speed reaches the spin coating speed of 2000-3000rpm and stops accelerating. In one embodiment of the present application, the spin coating method is static spin coating, that is, the lead iodide precursor solution is first applied to the surface of the substrate, and then the rotation is started; due to the high viscosity of the lead iodide precursor solution, it is not convenient to extend during dynamic spin coating, so static spin coating is adopted. In one embodiment of the present application, the rotation speed is 2500rpm, the time is 30s, the acceleration is 1000rpm / s, and the annealing is performed at 70°C for 1min.
[0033] In step S2, the coating is spin coating, the spin coating speed is 2500-3000rpm, the time is 20-50s, the acceleration is 1000-1500rpm / s, the temperature of the second annealing treatment is 140-160°C, the time is 10-20min, and the humidity is 30-40%RH. In one embodiment of the present application, the spin coating method is dynamic spin coating, that is, the lead iodide precursor solution is applied to the surface of the substrate while rotating, the speed is 2700rpm, the time is 30s, the acceleration is 1000rpm / s, and then annealed at 150°C for 15min in a humidity environment of 30-40RH%. When the humidity is within 30-40RH%, the device performance is optimal; if the humidity is too high, the perovskite is easy to decompose.
[0034] In the present application, the lead iodide layer prepared by any of the above embodiments has a porous structure, a pore size range of 60-100nm, an average pore size of 75-85nm, and an average area porosity of 35-45%. The area porosity is the percentage of the area of pores contained per unit area, which can reflect the proportion of pore area per unit area on the surface of the lead iodide layer. The lead iodide layer has more pores on the surface, which is conducive to the penetration of ammonium salt solution.
[0035] The present application introduces succinamide into the lead iodide precursor solution to form NH···I hydrogen bonds, which can reduce the lead iodide nucleation barrier, thereby forming a porous lead iodide layer, so that subsequent ammonium salts can penetrate more fully. Different from the traditional layer-by-layer penetration of ammonium salts, the ammonium salt solution achieves omnidirectional diffusion and spatial confinement effects through a porous structure, effectively promoting the complete conversion of perovskite and obtaining the desired perovskite film, thereby improving the photoelectric conversion efficiency of perovskite devices and further improving the device efficiency of perovskite or crystalline silicon stacked solar cells.
[0036] The present application provides a perovskite layer, which can be prepared by the method for preparing a perovskite layer in any of the above embodiments.
[0037] In one embodiment of the present application, the perovskite layer is FA x MA 1-x PbX3, wherein 0≤x≤1, X can be one or more of the halogen elements Cl, Br, and I; specifically, the perovskite layer includes but is not limited to FAPbI3, FAPbBr3, FAPbCl3, MAPbI3, MAPbBr3, MAPbCl3, FAPbBrI2, FAPbClI2, FAPbIBr2, FAPbICl2, FAPbClIBr, MAPbBrI2, MAPbClI2, MAPbIBr2, MAPbICl2 or MAPbClIBr, etc. In one embodiment of the present application, the perovskite layer can be FAPb(I 0.83 Br 0.17 ) 3. In one embodiment of the present application, the thickness of the perovskite layer is 400-600 nm, the particle size range of the perovskite grains is 800-1200 nm, and the average particle size of the perovskite grains is 950-1050 nm.
[0038] The present application provides a photovoltaic device, comprising the perovskite layer in any one of the above embodiments.
[0039] In one embodiment of the present application, the photovoltaic device may be a perovskite solar cell, such as Figure 1 As shown, the perovskite solar cell includes, from bottom to top, a first electrode layer 1, a hole transport layer 2, a perovskite layer 3, an electron transport layer 4, a hole blocking layer 5 and a metal electrode 6. The first electrode layer 1 can be FTO or ITO, etc.; the hole transport layer 2 can be PTAA, MeO-2PACz or NiO x etc.; the perovskite layer 3 is produced by the methods of the following embodiments; the electron transport layer 4 can be PC61BM, C 60 etc.; the hole blocking layer 5 may be BCP etc.; the metal electrode 6 may be an Ag electrode, a Cu electrode etc. In one embodiment of the present application, the first electrode layer 1 is FTO, the hole transport layer 2 is MeO-2PACz, and the perovskite layer 3 is FAPb(I 0.83 Br 0.17 )3, the electron transport layer 4 is C 60 , the hole blocking layer 5 is BCP, and the metal electrode 6 is an Ag electrode.
[0040] In one embodiment of the present application, the preparation process of the perovskite solar cell can refer to Figure 2 , including: FTO glass cleaning, hole transport layer preparation, perovskite layer preparation, C 60Evaporation, hole blocking layer preparation and Ag electrode evaporation. Among them, the preparation of the perovskite layer is prepared by a two-step method, referring to Figure 3 , specifically including the preparation of a PbI2 layer and an ammonium salt layer. The prepared PbI2 layer has a porous structure, which is conducive to the penetration of ammonium salt.
[0041] The effect of the technical solution of this application is further illustrated below through specific examples.
[0042] Example 1 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0043] c. Preparation of PbI2 layer: 93.6 mg PbBr2, 601.6 mg PbI2, 5 mg FA, 5 mg RbCl and 0.25 mg succinamide were dissolved in 1 mL of a mixed solution of DMF and DMSO (the volume ratio of DMF to DMSO was 9:1), and heated at 60°C for 2 hours to fully dissolve. Static spin coating was performed on the MeO-2PACz substrate at a speed of 2500 rpm for 30 seconds, an acceleration of 1000 rpm / s, and annealing at 70°C for 1 minute.
[0044] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0045] e.C60 layer preparation: vacuum degree is less than 3×10 -4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0046] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0047] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0048] Example 2 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0049] c. Preparation of PbI2 layer: 93.6mg PbBr2, 601.6mg PbI2, 5mg FAI, 5mg RbCl and 0.50mg succinamide were dissolved in 1mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60℃ for 2 hours to fully dissolve. Static spin coating was performed on MeO-2PACz substrate at a speed of 2500rpm, a time of 30s, an acceleration of 1000rpm / s, and annealing at 70℃ for 1min.
[0050] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0051] e.C60 layer preparation: vacuum degree is less than 3×10 -4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0052] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0053] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0054] Example 3 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0055] c. Preparation of PbI2 layer: 93.6 mg PbBr2, 601.6 mg PbI2, 5 mg FAI, 5 mg RbCl and 0.75 mg succinamide were dissolved in 1 mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60°C for 2 hours to fully dissolve. Static spin coating was performed on the MeO-2PACz substrate at a speed of 2500 rpm for 30 seconds, an acceleration of 1000 rpm / s, and annealing at 70°C for 1 minute.
[0056] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0057] e.C60 layer preparation: vacuum degree is less than 3×10 -4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0058] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0059] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0060] Example 4 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0061] c. Preparation of PbI2 layer: 93.6 mg PbBr2, 601.6 mg PbI2, 5 mg FAI, 5 mg RbCl and 1.00 mg succinamide were dissolved in 1 mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60°C for 2 hours to fully dissolve. Static spin coating was performed on the MeO-2PACz substrate at a speed of 2500 rpm for 30 seconds, an acceleration of 1000 rpm / s, and annealing at 70°C for 1 minute.
[0062] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0063] e.C60 layer preparation: vacuum degree is less than 3×10 -4Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0064] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0065] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0066] Example 5 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0067] c. Preparation of PbI2 layer: 93.6 mg PbBr2, 601.6 mg PbI2, 5 mg FAI, 5 mg RbCl and 0.15 mg succinamide were dissolved in 1 mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60°C for 2 hours to fully dissolve. Static spin coating was performed on the MeO-2PACz substrate at a speed of 2500 rpm for 30 seconds, an acceleration of 1000 rpm / s, and annealing at 70°C for 1 minute.
[0068] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0069] e.C60 layer preparation: vacuum degree is less than 3×10-4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0070] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0071] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0072] Example 6 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0073] c. Preparation of PbI2 layer: 93.6mg PbBr2, 601.6mg PbI2, 5mg FAI, 5mg RbCl and 1.40mg succinamide were dissolved in 1mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60℃ for 2 hours to fully dissolve. Static spin coating was performed on MeO-2PACz substrate at a speed of 2500rpm, a time of 30s, an acceleration of 1000rpm / s, and annealing at 70℃ for 1min.
[0074] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0075] e.C60 layer preparation: vacuum degree is less than 3×10 -4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0076] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0077] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0078] Comparative Example 1 a. FTO glass cleaning: ultrasonically clean the FTO glass with detergent water, ultrapure water, and anhydrous ethanol for 10 minutes respectively, take it out with tweezers, and blow it dry with a nitrogen air gun; b. Preparation of hole transport layer: The cleaned and dried FTO glass was plasma cleaned (high-purity oxygen atmosphere, power 120W, 8min), and then placed in a glove box filled with nitrogen. MeO-2PACz (dissolved in chlorobenzene) 0.5mg / mL, 3000 rpm static spin coating, 30s, 2000rpm / s acceleration, 100℃ annealing for 10min, the film thickness was 15nm.
[0079] c. Preparation of PbI2 layer: 93.6 mg PbBr2, 601.6 mg PbI2, 5 mg FAI and 5 mg RbCl were dissolved in 1 mL DMF and DMSO mixed solution (the volume ratio of DMF to DMSO was 9:1), and heated at 60°C for 2 hours to fully dissolve. Static spin coating was performed on the MeO-2PACz substrate at a speed of 2500 rpm for 30 seconds, an acceleration of 1000 rpm / s, and annealing at 70°C for 1 minute.
[0080] d. Preparation of ammonium salt layer: 90 mg FAI, 9 mg MACl, and 9 mg MABr were dissolved in 1 mL isopropanol. Dynamic spin coating was performed on the prepared PbI2 layer at a speed of 2700 rpm for 30 s and an acceleration of 1000 rpm / s, and then annealed at 150°C for 15 min in a 30-40% RH humidity environment.
[0081] e.C60 layer preparation: vacuum degree is less than 3×10 -4 Pa started to heat the evaporation source, and after the temperature rose to 540°C, the evaporation and sample baffles were opened at a rate of 0.2Å / s. When the film thickness reached 30nm, the baffles were closed, and when the temperature dropped to 200°C, exhaust was started, and the sample was taken out and placed in a nitrogen glove box.
[0082] f. Preparation of BCP layer: Dissolve 0.5 mg BCP in 1 mL isopropanol and stir until completely dissolved. Perform dynamic spin coating on the C60 layer at a speed of 5000 rpm for 30 s and an acceleration of 2000 rpm / s, and then anneal at 70°C for 5 min.
[0083] g. Ag electrode preparation: vacuum degree is less than 3×10 -4 Pa, start heating the evaporation source, adjust the power to evaporate 20nm at 1Å / s, 40nm at 2Å / s, and 60nm at 3Å / s, with a total film thickness of 120nm. When the evaporation is completed, close all the baffles and start the pump stop. After the molecular pump is turned off, take out the sample.
[0084] Performance Testing (1) Scanning electron microscope (SEM) test The lead iodide layer and the perovskite layer in Example 3 and the comparative example were photographed using a scanning electron microscope (SEM), and the morphologies of the lead iodide layer and the perovskite layer were recorded. Figure 4-7 And Table 1-2.
[0085] Table 1 Morphology of lead iodide layer
[0086] Table 2 Morphology of perovskite layer
[0087] (2) Current density-voltage characteristic curve (JV) test The JV equipment was used to test the device performance. The specific parameters are shown in Table 3.
[0088] Table 3 Current density-voltage characteristic curve (JV) test results
[0089] Figure 4 3 is an electron microscope image of the lead iodide layer in Example 3. From the image, we can see that the lead iodide layer prepared from the lead iodide precursor solution to which 0.75 mg of succinamide is added has a porous structure.
[0090] Figure 4 This is an electron microscope image of the lead iodide layer in Comparative Example 1. From the image, we can see that the lead iodide layer prepared from the lead iodide precursor solution without adding succinamide is dense.
[0091] Therefore, according to Figure 4 , Figure 5 By comparing the data in Table 1, it can be seen that the lead iodide layer prepared from the lead iodide precursor solution with the addition of succinamide has a significant porous structure with a pore size range of 60-100 nm; while the lead iodide layer of Comparative Example 1 has a dense structure because succinamide is not added.
[0092] Figure 6 This is an electron microscope image of the perovskite grains in Example 3. From the image, we can see that the perovskite grain size of the perovskite layer prepared from the lead iodide precursor solution to which 0.75 mg of succinamide is added is larger, indicating that the perovskite conversion is better and the perovskite grain quality is higher.
[0093] Figure 7 This is an electron microscope image of the perovskite grains in Comparative Example 1. From the image, we can see that the perovskite grain size of the perovskite layer prepared from the lead iodide precursor solution without the addition of succinamide is relatively small, indicating that the perovskite conversion is poor.
[0094] Therefore, according to Figure 6 , Figure 7 By comparing the data in Table 2, it can be seen that the change in the morphology of the lead iodide layer caused by succinamide brings a gain effect for the subsequent penetration of ammonium salt solution and the conversion of perovskite, and the particle size range of perovskite is 800-1200nm.
[0095] The results of the JV performance tests of the embodiments and comparative example 1 are shown in Table 3. Compared with comparative example 1, the short circuit and fill factor of the embodiments are significantly improved, so the battery efficiency is also significantly improved, indicating that the photovoltaic device prepared by adding succinamide has better device performance.
[0096] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A method for preparing a perovskite layer, characterized in that: The preparation method comprises: S1, coating a lead iodide precursor solution on a substrate surface, and performing a first annealing treatment to prepare a lead iodide layer; S2, coating an ammonium salt solution on the lead iodide layer, and performing a second annealing treatment to obtain the perovskite layer; Wherein, the lead iodide precursor solution comprises succinamide, lead salt and solvent.
2. The method for preparing a perovskite layer according to claim 1, characterized in that: The concentration of the succinamide in the lead iodide precursor solution is 0.2-1.2 mg / mL.
3. The method for preparing a perovskite layer according to claim 1, characterized in that: The lead salt includes one or more of PbBr2, PbI2 and PbCl2; the solvent includes one or more of DMF, DMSO, tBP and NMP.
4. The method for preparing a perovskite layer according to claim 1, characterized in that: The lead iodide layer has a porous structure, and the average pore size is 75-85nm.
5. The method for preparing a perovskite layer according to claim 1, characterized in that: The ammonium salt solution includes one or more of formamidine iodide, methylammonium chloride, methylammonium iodide and methylammonium bromide.
6. The method for preparing a perovskite layer according to claim 1, characterized in that: In the step S1, the coating is spin coating, the rotation speed of the spin coating is 2000-3000 rpm, the time is 20-50 s, the acceleration is 1000-1500 rpm / s, and the temperature of the first annealing treatment is 60-80° C., and the time is 0.5-3 min.
7. The method for preparing a perovskite layer according to claim 1, characterized in that: In the step S2, the coating is spin coating, the rotation speed of the spin coating is 2500-3000 rpm, the time is 20-50 s, the acceleration is 1000-1500 rpm / s, and the temperature of the second annealing treatment is 140-160° C., and the time is 10-20 min.
8. A perovskite layer, characterized in that: The perovskite layer is prepared by the method for preparing a perovskite layer according to any one of claims 1 to 7.
9. The perovskite layer according to claim 8, characterized in that The perovskite layer is FA x MA 1-x PbX3, wherein 0≤x≤1, and X is one or more of the halogen elements Cl, Br and I; and the thickness of the perovskite layer is 400-600nm.
10. The perovskite layer according to claim 8, characterized in that The average particle size of the perovskite grains in the perovskite layer is 900-1100 nm.
11. A photovoltaic device, characterized in that: The photovoltaic device comprises the perovskite layer according to any one of claims 9-10.