Preparation method of oxidized icariin modified collagen composite bone scaffold

By oxidizing icariin and blending it with collagen, aminated mesoporous bioactive glass and Mg-MOF-74@MSiO2, a cross-linked oxidized icariin-modified collagen composite bone scaffold was formed to solve the problem It solves the problems of insufficient stability and release rate of existing bone scaffold materials, and achieves improved physical and chemical properties of the bone scaffold and enhanced bone regeneration ability.

CN118831202APending Publication Date: 2024-10-25SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311207196.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-19
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing bone scaffold materials have deficiencies in stability and release rate, resulting in low cytotoxicity and low bioavailability, making it difficult to effectively promote bone repair in the long term.

Method used

Icariin was oxidized with sodium periodate to form oxidized icariin, which was introduced into collagen, aminated mesoporous bioactive glass and Mg-MOF-74@MSiO2 by dipping method, blended and freeze-dried to prepare The modified collagen composite bone scaffold is cross-linked through the Schiff base reaction of -CHO and -NH2 to improve the interface bonding strength and sustained release properties.

Benefits of technology

The prepared oxidized icariin-modified collagen composite bone scaffold has better physical and chemical properties, osteoconductivity, vascularization and anti-inflammatory properties, can slowly release active substances, improve bone formation and vascularization capabilities, and enhance bone regeneration potential. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a preparation method of an oxidized icariin modified collagen composite bone scaffold, which comprises the following steps: firstly, oxidizing o-dihydroxy in an icariin glycoside structure by sodium periodate to obtain oxidized icariin; and then introducing the oxidized icariin into a collagen composite bone scaffold (collagen-aminated mesoporous bioactive glass-mesoporous silica coated Mg-MOF-74) through an impregnation method to prepare the modified collagen composite bone scaffold. The oxidized icariin in the prepared modified collagen composite bone scaffold can be crosslinked with collagen, so that the interface bonding strength between the aminated mesoporous bioactive glass and the collagen is improved, and the scaffold has better physical and chemical properties and osteoconductivity; and the material can also cooperate with the Mg-MOF-74 coated with mesoporous silica to improve the osteogenesis, vascularization and anti-inflammatory performance of the stent. In addition, the raw materials are low in cost, and the preparation method is simple. Therefore, the stent has good application potential in the field of bone tissue engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an oxidized icariin-modified collagen composite bone scaffold, and belongs to the field of biomedical materials. Background Art

[0002] Bone defects are mainly treated by transplanting bone scaffolds. It is well known that the bone repair process in the body needs to go through three stages: inflammation, bone formation and bone remodeling. Therefore, the ideal bone scaffold should have suitable mechanical properties, a connected porous structure, good hydrophilicity, anti-degradation ability and osteoconductivity; more importantly, the scaffold also needs to have osteogenesis, vascularization and anti-inflammatory capabilities to enhance bone regeneration. For the research on bone scaffold materials, the current eye-catching trend is to mimic the composition of natural bones.

[0003] Natural bone is a composite material composed of an organic phase (mainly collagen), an inorganic non-metallic phase (mainly hydroxyapatite), and trace elements (Mg content is the highest). Collagen, as the main organic component in natural bone, provides elasticity and toughness to natural bone. It has good biocompatibility and biodegradability as an organic component of bone scaffolds. For inorganic non-metallic components, bioactive glass has better bioactivity than hydroxyapatite. Among them, mesoporous bioactive glass has a larger pore volume and specific surface area, which can accelerate the formation of hydroxyapatite mineralization, thereby significantly improving bone repair ability, but the interface bonding strength between it and collagen is insufficient. Trace element Mg 2+ It has the ability to improve scaffold bone formation, vascularization and anti-inflammatory ability. In view of this, Mg-MOF-74 with high specific surface area and adjustable pore structure has been used to improve osteogenic activity, vascularization and drug loading. It can be seen that Mg-MOF-74 can be regarded as Mg 2+ However, the stability of Mg-MOF-74 in PBS is low, which will lead to the 2+ If the release is too fast, it may cause cytotoxicity and fail to exert long-term effect. The strategy of coating the surface of Mg-MOF-74 with a mesoporous silica shell to obtain Mg-MOF-74@MSiO2 can improve its stability and slow down the release of Mg. 2+ The release rate of Mg-MOF-74@MSiO2 is better than that of Mg-MOF-74@MSiO2 in promoting cell proliferation.

[0004] Growth factors, as one of the components of bone tissue engineering, are often introduced into bone scaffolds to improve the bone repair performance of bone scaffolds, such as the commonly used vascular endothelial growth factor and bone morphogenetic protein-2, which can induce vascularization, activate osteogenesis-related signaling pathways, and ultimately promote bone regeneration. However, these growth factors are expensive, have poor stability, are easy to change, and have low bioavailability. Therefore, it is a current trend to replace growth factors with low-cost bioactive substances. As the main bioactive component of the traditional Chinese medicine epimedium, icariin has the characteristics of simple extraction process, wide source, and low cost. In addition, icariin also has significant osteogenic, angiogenic and anti-inflammatory effects. However, icariin, like other drugs, has the disadvantages of low bioavailability and short half-life (1-2 hours). The bone repair process takes a long time (3-6 months), and the drug needs to be released into the surrounding tissues for a long time and stably. In general, the sustained release of icariin in bone scaffolds is the key to exerting its functions such as osteogenic.

[0005] In order to solve the above problems, the present invention uses sodium periodate to oxidize the ortho-dihydroxyl group of the glycoside part of icariin to obtain oxidized icariin with -CHO, and then introduces the oxidized icariin into the collagen composite bone scaffold (COL-BG-MOF) prepared by blending collagen, amino mesoporous bioactive glass (BG-NH2) and Mg-MOF-74@MSiO2 and freeze-drying by impregnation. Oxidized icariin can cross-link collagen, improve the interface binding between BG-NH2 and collagen and slow down the release rate of oxidized icariin in COL-BG-MOF through the Schiff base reaction between -CHO and -NH2; in addition, oxidized icariin can also act as a "growth factor" to synergistically improve the bone formation, vascularization and anti-inflammatory properties of the scaffold with Mg-MOF-74@MSiO2. Finally, an oxidized icariin-modified collagen composite bone scaffold with both osteogenesis, vascularization and anti-inflammatory properties is prepared.

[0006] In summary, the present invention discloses a method for preparing an oxidized icariin-modified collagen composite bone scaffold, which can not only slowly release oxidized icariin, have better physicochemical properties and osteoconductivity, but also have bone formation, vascularization and anti-inflammatory properties, and has potential for application in bone tissue engineering. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing an oxidized icariin-modified collagen composite bone scaffold. The method of the present invention can not only ensure the structural integrity of icariin but also enable it to play the role of "growth factor", cross-linking agent and interface phase. The modified collagen composite bone scaffold obtained by combining it into a collagen composite bone scaffold can not only slowly release oxidized icariin, have better physical and chemical properties and osteoconductivity, but also have the properties required for bone scaffolds such as bone formation, vascularization and anti-inflammation.

[0008] The present invention provides, on one hand: A method for preparing an oxidized icariin-modified collagen composite bone scaffold comprises the following steps: (1) adding sodium periodate solution to icariin solution for oxidation reaction, then adding ethylene glycol to terminate the reaction, and then purifying and freeze-drying to obtain oxidized icariin; (2) BG-NH2 and Mg-MOF-74@MSiO2 were added to the collagen solution for blending, and then freeze-dried to obtain COL-BG-MOF; (3) After COL-BG-MOF is modified by immersing it in an oxidized icariin solution, it is washed and freeze-dried to obtain an oxidized icariin-modified collagen composite bone scaffold.

[0009] The preparation method is characterized in that in step (1), the sodium periodate solution is a solution obtained by dissolving 8-320 mg of sodium periodate in 2-16 mL of water, the icariin solution is a solution obtained by dissolving 10-80 mg of icariin in 20-160 mL of ethanol aqueous solution, the amount of ethylene glycol used is 1-4 mL, the oxidation reaction conditions are stirring at 15-35° C. and in the dark for 12-48 hours, and the termination reaction conditions are stirring at 15-35° C. and in the dark for 0.5-2 hours.

[0010] The preparation method is characterized in that in step (1), the purification process is to first place the obtained product in a 300-500 Da dialysis bag, and then dialyze it in 4-35° C. water for 3-4 days, and change the water every 4-6 hours.

[0011] The preparation method is characterized in that in step (2), the collagen solution is a solution formed by dissolving collagen in an acetic acid aqueous solution at 3-5°C, wherein the collagen includes any one or more of fetal bovine skin collagen, pig skin collagen, bovine Achilles tendon collagen, sheep skin collagen, and fish skin collagen.

[0012] The preparation method is characterized in that in step (2), the mass ratio of the collagen, the amino-modified mesoporous bioactive glass and the mesoporous silica-coated Mg-MOF-74 is 100~800:200~1600:10~80.

[0013] The preparation method is characterized in that in step (2), the mass ratio of the collagen, the amino-modified mesoporous bioactive glass and the mesoporous silica-coated Mg-MOF-74 is 10:20:1.

[0014] The preparation method is characterized in that in step (3), the oxidized icariin solution is prepared by dissolving oxidized icariin in an ethanol aqueous solution to obtain a solution with a concentration of 0 to 3 mg / mL, and the modification condition is stirring at 3 to 5°C for 12 to 48 hours.

[0015] The preparation method is characterized in that the key performance indicators of the oxidized icariin-modified collagen composite bone scaffold are as follows: (1) Evaluation of cross-linking degree: thermal denaturation temperature is 76.7±4.5℃; (2) Mechanical properties evaluation: compressive strength is 0.20±0.05 MPa, Young's modulus is 0.29±0.07 MPa; (3) Porous structure evaluation: The porosity was 60.5±5.4%, and the oxidized icariin-modified collagen composite bone scaffold had interconnected macropores of 100-200 μm; (4) Hydrophilicity evaluation: water contact angle is 25.9±2.9°, water absorption rate is 3138.8±373.4%; (5) Evaluation of enzyme degradation resistance: After 14 days of treatment with 1 U / mL type I collagenase solution, the degradation rate was 42.2±10.1%; (6) Evaluation of bone conduction performance: After 14 days of SBF treatment, the in vitro mineralization rate was 121.6±9.2%; (7) Cytocompatibility evaluation: After 5 days of co-culture of cells with sample extract, the relative cell proliferation rate was 123.7±10.0% and the cytotoxicity was level 0; (8) Evaluation of osteogenic activity: After 7 days of induction of cells with sample extract, the alkaline phosphatase activity was 0.28±0.06nm / min. After 14 days of induction of cells with sample extract, the color of alkaline phosphatase and alizarin red staining deepened. (9) Evaluation of vascularization performance: After 24 hours of co-culture of sample extract and cells, the scratch was almost completely closed, and a large number of cells migrated from the upper surface of the transwell chamber membrane to the lower surface of the membrane; (10) Evaluation of anti-inflammatory properties: After 24 hours of co-culture of the sample extract with cells, the concentrations of tumor necrosis factor-α (TNF-α) and were 381.55±7.76 pg / mL, and the concentration of interleukin-6 (IL-6) was 423.45±5.52 pg / mL;

[0016] The oxidized icariin prepared by the preparation method.

[0017] The oxidized icariin-modified collagen composite bone scaffold prepared by the preparation method.

[0018] The application of the oxidized icariin modified collagen composite bone scaffold in the field of bone tissue engineering.

[0019] Another aspect of the present invention provides the oxidized icariin prepared in step (1) of the preparation method of the present invention.

[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) Enhanced physical and chemical properties: Oxidized icariin acts as a cross-linking agent and an interfacial phase, which can enhance the ability of the triple helix structure of collagen in the bone scaffold to resist high temperature without being destroyed, the ability of the bone scaffold to better maintain and restore its morphology after being stressed, and the ability to hinder collagenase from entering the enzyme cleavage site on the bone scaffold, thereby improving the thermal stability, mechanical properties and resistance to enzyme degradation of the bone scaffold; (2) Improved bone conductivity: The negative charge of oxidized icariin is Ca 2+ The deposition of hydroxyapatite provides more binding sites, which is beneficial to the formation of hydroxyapatite, thereby enhancing the in vitro mineralization ability of the bone scaffold, that is, improving the osteoconductivity; (3) Oxidized icariin can be slowly released: Oxidized icariin can be loaded through the mesoporous adsorption and electrostatic interaction of BG-NH2 in the bone scaffold. In addition, -CHO in oxidized icariin can react with BG-NH2 and -NH2 on collagen to undergo Schiff base reaction, that is, the scaffold can also load oxidized icariin through chemical bonding, so that the oxidized icariin in the scaffold can be slowly released; (4) Oxidized icariin has multifunctionality: -CHO in oxidized icariin can react with -NH2 on collagen and BG-NH2 to undergo Schiff base reaction, which can not only act as a cross-linking agent to cross-link collagen and as an interface phase to promote the interface between BG-NH2 and collagen, but also act as a "growth factor" to synergize with Mg-MOF-74@MSiO2 to improve the bone formation, vascularization and anti-inflammatory properties of the scaffold; (5) Excellent cell compatibility: Oxidized icariin is used as the cross-linking agent of COL-BG-MOF. Oxidized icariin itself has good cell compatibility, which compensates for the negative effects of -CHO to a certain extent. The cytotoxicity of the oxidized icariin-modified collagen composite bone scaffold prepared by the present invention is level 0, which meets the use requirements of bone tissue engineering scaffolds. (6) Excellent in vitro osteogenesis, vascularization and anti-inflammatory properties: The icariin glycoside part has little effect on its bone repair performance, so oxidized icariin retains the bone repair-promoting property of icariin, allowing it to synergistically improve the bone formation, vascularization and anti-inflammatory properties of the scaffold with Mg-MOF-74@MSiO2; (7) The preparation process is simple and safe: the raw materials involved are low-cost, the preparation method is simple, and the reagents and reaction processes used in the preparation process are safe and environmentally friendly; (8) Adjustable performance: According to the performance requirements of the material, by controlling the reaction conditions (such as material ratio, temperature, time, etc.), oxidized icariin with different oxidation degrees can be prepared to adjust the performance of the scaffold. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 4 is the Fourier transform infrared spectra of the collagen composite bone scaffold modified with oxidized icariin of different concentrations in Example 1 of the present invention;

[0022] Figure 2 The alkaline phosphatase (ALP) activity of bone marrow mesenchymal stem cells (BMSCs) induced by the bone scaffold extract in Example 1 of the present invention after 7 days;

[0023] Figure 3 This is a representative picture of the ALP and Alizarin Red S (ARS) staining experiment after the bone scaffold extract induced BMSCs cells for 14 days in Example 1 of the present invention;

[0024] Figure 4 Representative images of the scratch and Transwell experiments of the cells after the bone scaffold extract and human umbilical vein endothelial cells (HUVEC) were co-cultured for 24 hours in Example 1 of the present invention;

[0025] Figure 5 The concentrations of TNF-α and IL-6 after the bone scaffold extract and Raw264.7 cells (stimulated with lipopolysaccharide (LPS)) were co-cultured for 24 hours in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with specific examples and accompanying drawings, but the protection scope of the present invention is not limited to the following examples. Unless otherwise specified, the reagents and raw materials used are commercially available.

[0027] BG-NH2 was prepared with reference to the existing technology (Zarghami V, Ghorbani M, Bagheri KP, et al. In vitro bactericidal and drug release properties of vancomycin-aminosurface functionalized bioactive glass nanoparticles[J]. Materials Chemistryand Physics, 2020, 241: 122423.).

[0028] Mg-MOF-74@MSiO2 was prepared with reference to the prior art (F. Li, Y. Chen, M. Gong, et al. Core-shell structure Mg-MOF-74@MSiO2 with mesoporous silica shell having efficiently sustained release ability of magnesium ions potential for bonerepair application, Journal of Non-Crystalline Solids 600 (2023).).

[0029] Example 1 Preparation of Icariin Oxide Modified Collagen Composite Bone Scaffold (1) Preparation of oxidized icariin: Weigh 20 mg of icariin in 40 mL of ethanol-water solution (50 vol%), sonicate until icariin is completely dissolved and the solution is clear to obtain solution A; add 32 mg of sodium periodate to 4 mL of deionized water, sonicate until completely dissolved to obtain solution B; then add B to A in a dark environment at 20°C, stir and react for 24 hours; then add 1 mL of ethylene glycol, stir in a dark environment for 1 hour to terminate the reaction; then place the obtained product in a 300 Da dialysis bag, dialyze in deionized water at 20°C for 3 days, and change the deionized water every 4 hours; finally, freeze-dry to obtain oxidized icariin; (2) Preparation of COL-BG-MOF: 200 mg of collagen was added to 40 mL of acetic acid aqueous solution (0.5 mol / L) and stirred at 4°C until the collagen was completely dissolved. Next, 400 mg of BG-NH2 and 20 mg of Mg-MOF-74@MSiO2 were added to the solution and stirred at 4°C for 4 hours until the solution was evenly dispersed. The obtained solution was then poured into a mold and freeze-dried to obtain COL-BG-MOF. Among them, the composite bone scaffold without the addition of Mg-MOF-74@MSiO2 was COL-BG. (3) Preparation of collagen composite bone scaffolds modified with icariin: Weigh 10, 20, 40, and 60 mg of icariin in 20 mL of ethanol aqueous solution (50 vol%), and ultrasonicate until the icariin is completely dissolved and the solution is clear to obtain solution C; 40 mg of COL-BG-MOF scaffold is completely immersed in 20 mL of solution C, and stirred for reaction at 4 °C for 24 h; finally, the modified scaffold is taken out and washed with deionized water, and freeze-dried to obtain collagen composite bone scaffolds modified with icariin of different concentrations (COL-BG-MOF-0.5, COL-BG-MOF-1, COL-BG-MOF-2, and COL-BG-MOF-3); among them, the COL-BG-MOF-0.5 scaffold modified with 10 mg of icariin was selected as the preferred group for subsequent experiments.

[0030] Example 2 Results and Discussion like Figure 1 As shown in the figure, the Fourier transform infrared spectra of all bone scaffolds showed absorption peaks reflecting the triple helical structure of type I collagen. Specifically, the amide I band at 1652 cm -1 A strong absorption peak appeared at 1545 cm, representing the bending vibration of NH and the stretching vibration of C=O and CN; -1 The amide II band at 1236 cm is attributed to the bending vibration of NH and the stretching vibration of CN; -1 The absorption peak of amide III proves the existence of amide III band, which is caused by CN stretching vibration and NH bending vibration of amide connection and -CH2 swinging vibration of glycine backbone and proline side chain group; the characteristic absorption peak of -OH and -NH2 of molecular side chain appears at about 3340 cm -1 and 2963 cm -1 , corresponding to the amide A band and the amide B band, respectively. This indicates that the interaction between the other components and collagen does not affect the structural integrity of collagen. At the same time, after the introduction of oxidized icariin into the scaffold, the absorption peak intensity of the amide I, II, and III bands of the scaffold was slightly reduced, confirming the generation of cross-linking. In addition, after the compounding of BG-NH2, the infrared spectrum of the scaffold also showed Si-O-Si characteristic absorption peaks, confirming the successful preparation of the composite scaffold.

[0031] like Figure 2 As shown in the figure, the ALP activity of BMSCs cells induced by bone scaffold extract after 7 days showed that the ALP activity of cells incubated with COL-BG-MOF scaffold introduced with Mg-MOF-74@MSiO2 was significantly increased compared with that of COL-BG scaffold, which was attributed to the Mg 2+It has a significant effect on promoting bone differentiation. After the introduction of oxidized icariin into the COL-BG-MOF scaffold, the ALP activity was further increased. The results showed that the scaffold containing Mg-MOF-74@MSiO2 and oxidized icariin can promote the ALP expression of BMSCs cells, and further confirmed that the oxidized icariin modified collagen composite bone scaffold has a good potential to promote bone formation; like Figure 3 As shown in the figure, the ALP and ARS staining results of the bone scaffold extract induced BMSCs cells for 14 days showed that the color of the collagen composite scaffold containing Mg-MOF-74@MSiO2 and oxidized icariin was the darkest, that is, the scaffold can significantly promote the differentiation of BMSCs into osteoblasts, which further confirmed that the oxidized icariin modified collagen composite bone scaffold has better bone regeneration ability; like Figure 4 As shown in the figure, the results of cell scratch and Transwell experiments after 24 hours of co-culture of bone scaffold extract and HUVEC cells showed that all groups showed cell migration, and the cell migration of the scaffold group was much better than that of the control group. It is worth noting that the collagen composite scaffold containing Mg-MOF-74@MSiO2 and oxidized icariin had the best cell migration ability at 24 hours, the scratch was almost completely closed, and the number of cells migrating from the upper surface of the membrane to the lower surface was significantly more than that of the other groups, that is, the oxidized icariin modified collagen composite bone scaffold has better vascularization ability; like Figure 5 As shown in the figure, the concentrations of tumor necrosis factor-α (TNF-α) and interleukin-6 (IL-6) after 24 hours of co-culture of bone scaffold extract with Raw264.7 cells (after LPS stimulation) showed that the concentrations of TNF-α and IL-6 in the COL-BG-MOF treatment group were lower than those in the COL-BG-MOF treatment group, indicating that the scaffolds after adding Mg-MOF-74@MSiO2 had higher anti-inflammatory ability. In addition, the composite scaffold group containing Mg-MOF-74@MSiO2 and oxidized icariin further inhibited the expression of inflammatory factors, especially TNF-α, on the basis of COL-BG-MOF. Therefore, the introduction of Mg-MOF-74@MSiO2 and oxidized icariin into the collagen composite scaffold can synergistically reduce the expression of TNF-α and IL-6 in Raw264.7 cells induced by LPS, that is, the collagen composite bone scaffold modified with oxidized icariin has better anti-inflammatory properties.

[0032] Obviously, the above-mentioned embodiments are only preferred embodiments for explaining the present invention, and are not intended to limit the implementation methods. For those skilled in the art, different forms of changes or modifications can be made based on the above description, and these changes or modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing an oxidized icariin-modified collagen composite bone scaffold, characterized in that: The following steps are involved: (1) adding sodium periodate solution to icariin solution for oxidation reaction, then adding ethylene glycol to terminate the reaction, and then purifying and freeze-drying to obtain oxidized icariin; (2) adding amino-modified mesoporous bioactive glass and mesoporous silica-coated Mg-MOF-74 to the collagen solution for blending, and then freeze-drying to obtain a collagen composite bone scaffold; (3) After the collagen composite bone scaffold is immersed in an oxidized icariin solution for modification, the oxidized icariin-modified collagen composite bone scaffold is obtained through washing and freeze-drying.

2. The preparation method according to claim 1, characterized in that: In step (1), the sodium periodate solution is a solution obtained by dissolving 8-320 mg of sodium periodate in 2-16 mL of water, the icariin solution is a solution obtained by dissolving 10-80 mg of icariin in 20-160 mL of ethanol aqueous solution, the amount of ethylene glycol used is 1-4 mL, the oxidation reaction conditions are stirring at 15-35° C. and in the dark for 12-48 hours, and the termination reaction conditions are stirring at 15-35° C. and in the dark for 0.5-2 hours.

3. The preparation method according to claim 1, characterized in that: In step (1), the purification process is to place the obtained product in a 300-500 Da dialysis bag, dialyze it in 4-35° C. water for 3-4 days, and change the water every 4-6 hours.

4. The preparation method according to claim 1, characterized in that: In step (2), the collagen solution is a solution formed by dissolving collagen in an acetic acid aqueous solution at 3-5° C., wherein the collagen includes any one or more of fetal bovine skin collagen, pig skin collagen, bovine Achilles tendon collagen, sheep skin collagen, and fish skin collagen.

5. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the collagen, the amino-modified mesoporous bioactive glass and the mesoporous silica-coated Mg-MOF-74 is 100-800:200-1600:10-80.

6. The preparation method according to claim 5, characterized in that: In step (2), the mass ratio of the collagen, the amino-modified mesoporous bioactive glass and the mesoporous silica-coated Mg-MOF-74 is 10:20:

1.

7. The preparation method according to claim 1, characterized in that: In step (3), the oxidized icariin solution is prepared by dissolving oxidized icariin in an ethanol aqueous solution to obtain a solution with a concentration of 0 to 3 mg / mL, and the modification condition is stirring at 3 to 5°C for 12 to 48 hours.

8. Oxidized icariin prepared according to the preparation method according to any one of claims 1 to 3.

9. An oxidized icariin-modified collagen composite bone scaffold prepared according to the preparation method according to any one of claims 1 to 7.

10. Use of the oxidized icariin-modified collagen composite bone scaffold according to claim 9 in the field of bone tissue engineering.