Graphene slurry with high oil absorption value and low viscosity and preparation method thereof

By using specific viscosity reducing agents and process adjustments in graphene slurry, the problems of high viscosity and poor fluidity of graphene slurry are solved, the preparation of graphene slurry with high oil absorption value and low viscosity is achieved, and the conductive properties and flow are improved. sex.

CN118841207APending Publication Date: 2024-10-25JIANGSU SHANYUAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049536.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In the preparation of graphene slurry, the existing technology has high viscosity and poor fluidity, which affects production efficiency and reduces electrical conductivity. Adding too many additives will damage the electrical performance.

Method used

By using viscosity reducing agents with diamine groups, PPO groups and PEO groups, and adjusting the defects of graphene, combined with specific process conditions, a graphene slurry with high oil absorption value and low viscosity can be prepared to reduce the viscosity. And ensure conductive properties.

Benefits of technology

The viscosity of the graphene slurry is significantly reduced, the fluidity is improved, and the resistivity of the electrode sheet in the lithium battery negative electrode slurry is significantly improved, ensuring the improvement of the conductive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841207A_ABST
    Figure CN118841207A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of graphene slurry preparation, and particularly relates to high-oil-absorption low-viscosity graphene slurry and a preparation method thereof, and the technical key points are as follows: the high-oil-absorption low-viscosity graphene slurry comprises a pre-dispersion liquid and a viscosity reducer; wherein the pre-dispersion liquid comprises graphene, a dispersing agent and a solvent; the graphene slurry comprises the following components in percentage by mass: 0.5-6% of graphene, 0.5-3% of a dispersing agent, 0.05-2% of a viscosity reducer and the balance of a solvent, wherein the viscosity reducer comprises a diamine group, a PPO group and a PEO group, and the diamine group is grafted with the PPO group or the PEO group. The novel viscosity reducer and graphene with a certain defect degree are adopted, the graphene slurry is prepared by simply adjusting procedures, the viscosity of the graphene slurry is greatly reduced, the pipeline conveying and other process requirements of downstream customers are met, used equipment is conventional general equipment in the industry, the process steps are simple, and complex equipment and procedures are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of graphene slurry preparation, and particularly relates to a graphene slurry with high oil absorption value and low viscosity and a preparation method thereof. Background Art

[0002] Graphene is a carbon atom in the form of sp 2 Two-dimensional carbon nanomaterials with hexagonal honeycomb lattices composed of hybrid orbitals have excellent electronic, thermal and mechanical properties, and therefore have broad application prospects in new energy, electronic devices, biomedicine and other fields.

[0003] Since graphene with thin layers and good conductivity has a high specific surface area and high oil absorption value, when preparing graphene slurry, it has high viscosity and poor fluidity, which not only affects the production efficiency but also restricts the application of graphene slurry.

[0004] In the prior art, the fluidity of graphene slurry is usually improved by increasing the amount of additives such as dispersants. However, if the amount added is too high, it will affect the electrical properties of the graphene slurry, reduce the conductivity of downstream products, and the viscosity reduction ability is limited. Summary of the invention

[0005] The purpose of the present invention is to provide a low-viscosity graphene slurry with high oil absorption value and a preparation method thereof, and the fluidity of the graphene slurry is improved and the viscosity of the graphene slurry is reduced by adjusting the group of the viscosity reducing agent and the defect degree of the graphene, thereby ensuring the conductive performance of the graphene slurry.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] The present invention provides a graphene slurry with high oil absorption value and low viscosity, comprising a pre-dispersed liquid and a viscosity reducer;

[0008] Wherein, the pre-dispersion liquid comprises graphene, a dispersant and a solvent;

[0009] Calculated by mass percentage, the graphene slurry includes the following components:

[0010] Graphene 0.5-6%, dispersant 0.5-3%, viscosity reducer 0.05-2%, and the balance is solvent;

[0011] The viscosity reducer comprises a diamine group, a PPO group and a PEO group, and the diamine group is grafted with the PPO group or the PEO group.

[0012] Further, the general structural formula of the viscosity reducer is as follows:

[0013]

[0014] Wherein, R contains a PPO group and a PEO group, and the value range of n is a positive integer between 1 and 20.

[0015] Furthermore, the R group can be R1 or R2, and the general structural formula is as follows:

[0016]

[0017] Wherein, x and y are both positive integers between 1 and 50.

[0018] Furthermore, the viscosity reducing agent is obtained by grafting ethylenediamine onto PPO-PEO groups, and its structural formula is as follows:

[0019]

[0020] Wherein, x and y are both positive integers between 1 and 50.

[0021] Furthermore, the graphene defect degree I is determined according to the intensity ratio Id / Ig of the D peak and the G peak of the Raman spectrum, and the value range of the defect degree I is 0.8 to 1.5.

[0022] Furthermore, the amount of viscosity reducer added is calculated according to the following formula:

[0023]

[0024] Wherein, I is the defect degree of graphene, which is determined by the intensity ratio of D peak to G peak of Raman spectrum, Id / Ig, and the unit is 1;

[0025] S is the mass percentage of graphene in the graphene slurry, in %;

[0026] M is the mass percentage of the viscosity reducer in the graphene slurry, in %;

[0027] B is the adjustment constant, the unit is 1, and the value range is 8≤B≤40.

[0028] Further, the graphene is subjected to redox modification.

[0029] Furthermore, the dispersant is any one of polyvinyl pyrrolidone, polyether surfactants, polyacrylic acid surfactants, polyurethane surfactants, tannic acid or sodium carboxymethyl cellulose.

[0030] Furthermore, graphene meets the following conditions: particle size distribution, D50 ≤ 100 μm; specific surface area ≥ 400 m 2 / g; oil absorption value ≥2000ml / 100g.

[0031] The present invention also provides a method for preparing a graphene slurry with high oil absorption value and low viscosity, comprising the following steps:

[0032] Stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0033] Under the first parameter condition, grinding or shearing the pre-dispersed liquid to obtain an initial slurry;

[0034] A viscosity reducing agent is added to the initial slurry, and the slurry is ground or sheared under the second parameter condition to obtain the graphene slurry with a set viscosity and particle size.

[0035] Furthermore, the first parameter condition includes a rotation speed of 300 to 1000 rpm and a pump pressure of 0.1 to 0.3 bar.

[0036] Furthermore, the second parameter conditions include a rotation speed of 50 to 400 rpm and a pump pressure of 0.1 to 0.3 bar.

[0037] Furthermore, the viscosity is set to ≤2000 mPa.s at 10 inverse seconds; and the particle size D50 is set to 1-5 um.

[0038] In summary, the present invention has the following beneficial effects:

[0039] The present invention adopts a new viscosity reducing agent and graphene with a certain degree of defects, and the viscosity of the graphene slurry prepared by simply adjusting the process is greatly reduced. The graphene slurry prepared by the viscosity reducing agent, graphene and process has significantly improved conductivity compared with the graphene slurry prepared by low specific surface area and low oil absorption value powder, which is reflected by the pole sheet resistivity of the negative electrode slurry in the lithium battery; the graphene slurry prepared by the low specific surface area and low oil absorption value powder has a pole sheet resistivity of more than 100Ω.cm in the silicon-based main material, while the graphene slurry prepared by the high specific surface area and high oil absorption value graphene has a pole sheet resistivity of less than 5Ω.cm, and the conductivity is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a comparison chart of the viscosity of the final product in the embodiment;

[0041] Figure 2 This is a comparison chart of the viscosity of the grinding discharge in the embodiment;

[0042] Figure 3 This is a comparison diagram of the resistivity of the electrode sheets of the embodiment;

[0043] Figure 4 It is a comparison chart of the defect degree of Example 1 and Comparative Example 3. DETAILED DESCRIPTION

[0044] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, a high oil absorption and low viscosity graphene slurry and a preparation method thereof proposed in accordance with the present invention, its specific implementation method, characteristics and effects are described in detail as follows.

[0045] The sources of raw materials used in this specific implementation are as follows:

[0046] Graphene: Changzhou Sixth Element Technology Co., Ltd.

[0047] Expanded graphite: Qingdao Tianshengda Graphite Co., Ltd.;

[0048] Ethanolamine: Nanjing Chemical Reagent Co., Ltd.;

[0049] Polyvinylpyrrolidone (PVP): Shanghai Naxi New Material Technology Co., Ltd. K30;

[0050] Tannic acid: Xinyang Mufan Technology Biological Co., Ltd.;

[0051] Sodium carboxymethyl cellulose: Shanghai Shenguang Food Chemicals Co., Ltd.;

[0052] Polyurethane dispersant: Evonik Specialty Chemicals (Shanghai) Co., Ltd.

[0053] Polyether dispersant: Clariant Chemicals (China) Co., Ltd., TC109.

[0054] This specific embodiment provides a high oil absorption and low viscosity graphene slurry and a preparation method thereof, which adopts diamine grafted PPO group or PEO group to prepare a new viscosity reducer, and achieves the viscosity reduction effect on the slurry by adjusting different groups; selects graphene with high conductivity, high specific surface area and high oil absorption value with appropriate defect degree to prepare graphene slurry; finally, the viscosity of the graphene slurry is further adjusted through the process.

[0055] This specific embodiment provides a graphene slurry with high oil absorption value and low viscosity, including a pre-dispersion liquid and a viscosity reducer;

[0056] Wherein, the pre-dispersion liquid comprises graphene, a dispersant and a solvent;

[0057] Calculated by mass percentage, the graphene slurry includes the following components:

[0058] Graphene 0.5-6%, preferably 2.5-4%; viscosity reducer 0.05-2%; dispersant 0.5-3%, preferably 0.5-2%, and the balance is solvent;

[0059] The viscosity reducer comprises a diamine group, a PPO group and a PEO group, and the diamine group is grafted with the PPO group or the PEO group.

[0060] In the viscosity reducer of the diamine grafted PPO group or PEO group provided in this specific embodiment, PPO (polyoxypropylene) is generally formed by oxidative polymerization of propylene, and its main part is composed of [-CH2-CH(CH3)-O-] units; PEO (polyoxyethylene) is formed by oxidative polymerization of ethylene, and its main part is composed of [-CH2-CH2-O-] units; diamines such as ethylenediamine (EDA) have a molecular formula of H2N-CH2-CH2-NH2, have two amino groups, and can react with the end or side chain of the polymer chain to form a grafted structure; the above structure combines the hydrophobicity of PPO, the hydrophilicity of PEO and the multifunctionality of diamine, so that the viscosity reducer can be connected to the groups at the defects of graphene (such as oxygen-containing, nitrogen-containing functional groups, methyl groups, etc.), bringing a higher degree of freedom, thereby effectively reducing the viscosity of the graphene slurry.

[0061] Specifically, the general structural formula of the viscosity reducer provided in this embodiment is as follows:

[0062]

[0063] Among them, R contains PPO group and PEO group;

[0064] The value range of n is a positive integer between 1 and 20, and preferably a positive integer between 2 and 5.

[0065] Furthermore, the R group can be R1 or R2, and the general structural formula is as follows:

[0066]

[0067] Wherein, x and y are both positive integers between 1 and 50.

[0068] More preferably, the viscosity reducer is obtained by grafting ethylenediamine onto PPO-PEO groups, called SYJ, and its structural formula is as follows:

[0069]

[0070] Wherein, x and y are both positive integers between 1 and 50.

[0071] The graphene defect degree I provided in this specific embodiment is determined according to the intensity ratio Id / Ig of the D peak and the G peak of the Raman spectrum, and the defect degree I ranges from 0.8 to 1.5.

[0072] Specifically, in the Raman spectrum of graphene, the appearance of the D peak is related to the defect density. By measuring the intensity ratio of the D peak and the G peak, the defect density can be quantitatively estimated, and then the content of the groups (such as oxygen-containing, nitrogen-containing functional groups, methyl groups, etc.) at the graphene defects can be judged; if the defect rate is too low, the interaction force between graphene and the viscosity reducer will be reduced, and the purpose of reducing the viscosity of the graphene slurry and improving the fluidity will not be achieved; if the defect rate is too high, it means that there are too many graphene defects, which will cause the conductivity of graphene to drop seriously, and the interaction force with the viscosity reducer is too high, which will increase the viscosity of the graphene slurry.

[0073] In some preferred embodiments, the amount of viscosity reducer added is calculated according to the following formula:

[0074]

[0075] Wherein, I is the defect degree of graphene, which is determined by the intensity ratio of D peak to G peak of Raman spectrum, Id / Ig, and the unit is 1;

[0076] S is the mass percentage of graphene in the graphene slurry, in %;

[0077] M is the mass percentage of the viscosity reducer in the graphene slurry, in %;

[0078] B is the adjustment constant, the unit is 1, and the value range is 8≤B≤40.

[0079] In this specific embodiment, the dosage of the viscosity reducer is limited by the defect degree of graphene, which can ensure that the connection rate between graphene and the viscosity reducer SYJ is within an appropriate range, effectively reduce the viscosity of the graphene slurry, greatly improve the fluidity of the graphene slurry, and avoid the addition of too much viscosity reducer, which affects the conductive properties of the graphene slurry.

[0080] Specifically, the value of B is obtained by fitting experimental data, and is more preferably 10-30.

[0081] In this specific embodiment, the graphene is redox modified.

[0082] Specifically, the method of redox modification of graphene is: using a strong oxidant, such as a strong acid, to oxidize the graphene, and then thermally reducing it at high temperature.

[0083] In this specific embodiment, the dispersant is any one of polyvinyl pyrrolidone, polyether surfactants, polyacrylic acid surfactants, polyurethane surfactants, tannic acid or sodium carboxymethyl cellulose.

[0084] In this specific embodiment, the graphene meets the following conditions: particle size distribution, D50 ≤ 100 μm; specific surface area ≥ 400 m 2 / g; oil absorption value ≥2000ml / 100g.

[0085] Specifically, when the specific surface area of ​​graphene is greater than 400m 2 / g, and when the oil absorption value is greater than 2000ml / 100g, the dispersion performance of graphene is poor. The viscosity reducer provided in this specific embodiment can greatly improve the fluidity of the graphene slurry.

[0086] This specific embodiment also provides a method for preparing a graphene slurry with high oil absorption value and low viscosity, comprising the following steps:

[0087] S1, stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0088] S2. Grinding or shearing the pre-dispersed liquid under the first parameter condition to obtain an initial slurry;

[0089] S3, adding a viscosity reducing agent to the initial slurry, and grinding or shearing under the second parameter condition to obtain the graphene slurry with a set viscosity and particle size.

[0090] In some preferred embodiments, the first parameter condition includes a rotation speed of 300-1000 rpm and a pump pressure of 0.1-0.3 bar.

[0091] In some preferred embodiments, the second parameter condition includes a rotation speed of 50 to 400 rpm and a pump pressure of 0.1 to 0.3 bar.

[0092] In some preferred embodiments, the viscosity is set to ≤2000 mPa.s at 10 inverse seconds; and the particle size D50 is set to 1-5 um.

[0093] Example 1: A high oil absorption value and low viscosity graphene slurry and preparation method thereof

[0094] The present embodiment provides a graphene slurry with high oil absorption and low viscosity, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 96.1% deionized water and 0.15% viscosity reducer SYJ.

[0095] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0096] The method for preparing the graphene slurry with high oil absorption value and low viscosity provided in this embodiment comprises the following steps:

[0097] S1, stirring and pre-dispersing graphene, a dispersant and deionized water to obtain a pre-dispersed liquid;

[0098] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0099] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0100] Comparative Example 1:

[0101] The present embodiment provides a graphene slurry, including a pre-dispersion liquid. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 1.5% PVP dispersant and 95.5% deionized water.

[0102] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0103] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0104] S1, stirring and pre-dispersing graphene, a dispersant and deionized water to obtain a pre-dispersed liquid;

[0105] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain a graphene slurry.

[0106] Comparative Example 2:

[0107] The present embodiment provides a graphene slurry, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 96.1% deionized water and 0.15% viscosity reducer SYJ.

[0108] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0109] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0110] S1, stirring and pre-dispersing graphene, dispersant, viscosity reducer SYJ and deionized water to obtain a pre-dispersion liquid;

[0111] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain a graphene slurry.

[0112] Example 2: A high oil absorption value and low viscosity graphene slurry and preparation method thereof

[0113] The present embodiment provides a graphene slurry with high oil absorption and low viscosity, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the pre-dispersion liquid includes the following components: 3% graphene, 0.75% PVP dispersant and 96.15% deionized water; the dosage of the viscosity reducer SYJ is 0.1% of the total mass of the pre-dispersion liquid.

[0114] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0115] The method for preparing the graphene slurry with high oil absorption value and low viscosity provided in this embodiment comprises the following steps:

[0116] S1, stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0117] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0118] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0119] Example 3: A high oil absorption value and low viscosity graphene slurry and preparation method thereof

[0120] The present embodiment provides a graphene slurry with high oil absorption and low viscosity, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 95.95% deionized water and 0.3% viscosity reducer SYJ.

[0121] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0122] The method for preparing the graphene slurry with high oil absorption value and low viscosity provided in this embodiment comprises the following steps:

[0123] S1, stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0124] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0125] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0126] Example 4: A high oil absorption value and low viscosity graphene slurry and preparation method thereof

[0127] The present embodiment provides a graphene slurry with high oil absorption and low viscosity, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the graphene slurry includes the following components: 2% graphene, 0.5% PVP dispersant, 97.37% deionized water, and 0.13% viscosity reducer SYJ.

[0128] Among them, the defect degree of graphene is I=Id / Ig=1.3; the oil absorption value is 3861ml / 100g.

[0129] The method for preparing the graphene slurry with high oil absorption value and low viscosity provided in this embodiment comprises the following steps:

[0130] S1, stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0131] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0132] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0133] Comparative Example 3:

[0134] The present embodiment provides a graphene slurry, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the pre-dispersion liquid includes the following components: 6% expanded graphite powder, 1.25% PVP dispersant and 92.6% deionized water; the dosage of the viscosity reducer SYJ is 0.15% of the total mass of the dispersion liquid.

[0135] The defect degree of the expanded graphite powder is I=Id / Ig=0.3; and the oil absorption value is 317 ml / 100 g.

[0136] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0137] S1, stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid;

[0138] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0139] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0140] Comparative Example 4:

[0141] The present embodiment provides a graphene slurry, including a pre-dispersion liquid and ethanolamine. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 96.1% deionized water, and 0.15% ethanolamine.

[0142] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0143] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0144] S1, stirring and pre-dispersing graphene, a dispersant and deionized water to obtain a pre-dispersed liquid;

[0145] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0146] S3. Add ethanolamine to the initial slurry, stir at a low speed of 300 rpm for 15 minutes, and obtain graphene slurry when the viscosity is stable.

[0147] Comparative Example 5:

[0148] A graphene slurry provided in this embodiment includes a pre-dispersion liquid and polyether TC109. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 96.1% deionized water, and 0.15% polyether TC109.

[0149] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0150] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0151] S1, stirring and pre-dispersing graphene, a dispersant and deionized water to obtain a pre-dispersed liquid;

[0152] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0153] S3. Add polyether TC109 to the initial slurry, stir at a low speed of 300 rpm for 15 minutes, and obtain graphene slurry when the viscosity is stable.

[0154] Comparative Example 6:

[0155] A graphene slurry provided in this embodiment includes a pre-dispersion liquid, polyether TC109 and ethanolamine. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 95.95% deionized water, 0.15% polyether TC109 and 0.15% ethanolamine.

[0156] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0157] The method for preparing the graphene slurry provided in this embodiment comprises the following steps:

[0158] S1, stirring and pre-dispersing graphene, a dispersant and deionized water to obtain a pre-dispersed liquid;

[0159] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0160] S3. Add ethanolamine and polyether TC109 to the initial slurry, stir at a low speed of 300 rpm for 15 minutes, and obtain graphene slurry when the viscosity is stable.

[0161] Comparative Example 7:

[0162] A kind of graphene slurry with high oil absorption value and low viscosity and preparation method thereof

[0163] The present embodiment provides a graphene slurry with high oil absorption and low viscosity, including a pre-dispersion liquid and a viscosity reducer SYJ. Calculated by mass percentage, the graphene slurry includes the following components: 3% graphene, 0.75% PVP dispersant, 96.1% N-methylpyrrolidone (NMP), and 0.15% viscosity reducer SYJ.

[0164] Among them, the defect degree of graphene is I=Id / Ig=1; and the oil absorption value is 3190ml / 100g.

[0165] The method for preparing the graphene slurry with high oil absorption value and low viscosity provided in this embodiment comprises the following steps:

[0166] S1, stirring and pre-dispersing graphene, a dispersant and NMP to obtain a pre-dispersed liquid;

[0167] S2. Grind the pre-dispersed liquid with a sand mill at a rotation speed of 800 rpm and a pump pressure of 0.2 bar until D50 is 3 μm to obtain an initial slurry;

[0168] S3. Add viscosity reducer SYJ to the initial slurry, stir at a low speed of 300 rpm for 15 min, and obtain graphene slurry when the viscosity is stable.

[0169] The preparation parameters and performance test results of the graphene slurries in Examples 1 to 4 and Comparative Examples 1 to 7 are summarized, and the results are shown in Table 1.

[0170] Among them, the test method of the electrode resistivity is: according to the formula, according to the mass ratio, silicon-based negative electrode material: sodium carboxymethyl cellulose (CMC): styrene-butadiene rubber emulsion (SBR): conductive agent (SW) = 91.95:2.55:3.5:2 are mixed, and then the mixed slurry is scraped to prepare an electrode (PET substrate), and after drying in a vacuum oven, the electrode is cut into a size of 4cm*4cm, and the electrode thickness is measured using an altimeter, and the electrode resistivity is tested using Suzhou Jingge ST2258C four-probe resistivity tester.

[0171] Viscosity test method: Use the DV2TRV viscometer produced by BROOKFIELD, USA. Pour the prepared sample into the matching test metal tube, rotate the lifting knob to slowly immerse the rotor in the liquid to be tested until the rotor liquid level mark (the groove or scale on the rotor rod) and the liquid surface are in the same plane. Select the 21# rotor, set the countdown program required for the test (usually 10 countdown seconds), and control the temperature during the test at 23±1℃.

[0172] Table 1. Preparation parameters and test results

[0173]

[0174]

[0175] According to the results in Table 1, the viscosity of the slurry with high viscosity and poor fluidity in Example 1 was reduced from 8447 to 350 mPa.s after the viscosity reducer SYJ was added, and the fluidity was improved, indicating that the viscosity reducer SYJ had a significant viscosity reduction effect.

[0176] Compared with the viscosity in Example 1 without adding the viscosity reducer SYJ, Comparative Example 1 shows that without adding the viscosity reducer SYJ, only increasing the amount of the dispersant PVP, the viscosity is slightly reduced, but the effect is not obvious, the viscosity is still very high, and the fluidity is still very poor.

[0177] Compared with Example 1, the addition process sequence of the viscosity reducer SYJ in Comparative Example 2 is different. In Comparative Example 2, the viscosity reducer SYJ is added during pre-dispersion. As a result, the viscosity of the discharge material after grinding is still very high, which is 7313 mPa.s. This shows that the viscosity reducer SYJ is not suitable for addition before grinding. The high shear force and grinding during the grinding process will destroy the interaction between the viscosity reducer SYJ and the groups at the graphene defects. If the molecular bond force between the oxygen-containing and nitrogen-containing groups at the graphene defects and the viscosity reducer SYJ, and the hydrogen bond force between the methyl groups at the graphene defects and the viscosity reducer SYJ are destroyed, the viscosity reducer SYJ cannot interact with the graphene, so that the graphene aggregates, resulting in an increase in viscosity.

[0178] Similarly, when the viscosity of the slurry prepared from the powder is different, the conductivity will also be different. The material with low viscosity and good fluidity will be better and more evenly dispersed in the subsequent application of the slurry, and it also ensures that the dispersion in the substrate is more uniform, with less agglomeration, the conductive network is relatively more complete, and the conductivity will be better, such as the comparison between Example 1 and Comparative Example 1.

[0179] Compared with Examples 2 and 3, Example 1 has different addition amounts of viscosity reducer SYJ, which are 0.15%, 0.1%, and 0.3%, respectively, showing different viscosity reduction effects. The more SYJ is added, the more obvious the viscosity reduction effect is. After adding a certain amount, it can even be like water. (In Examples 1, 2, and 3, I·S / M=20, 30, and 10, which meet the definition in the present invention).

[0180] In Example 4, compared with Example 1, the graphene defect degree is adjusted to Id / Ig=1.3, the oil absorption value is 3861ml / 100g, and the viscosity of the slurry is significantly higher after grinding. However, after adding the viscosity reducer SYJ, the viscosity reduction effect is very obvious and the fluidity is improved.

[0181] Compared with Example 1, in Comparative Example 3, the powder is adjusted to Id / Ig=0.3, and the oil absorption value is 317ml / 100g, so that the solid content can be higher, that is, the solid content of the conductive agent is 6%, and the dispersant increases by 1.25% year-on-year. The viscosity of the slurry after grinding is 2273mpa.s. After adding the viscosity reducer SYJ-0.15% (I·S / M=12), the defect degree does not meet the range specified by the present invention. The viscosity of the prepared graphene slurry is 2157mpa.s, with no obvious change. Therefore, the viscosity reducer SYJ has no obvious viscosity reducing effect on powders with low defect degrees.

[0182] This shows that the defect degree is small, the various groups are few, the viscosity reducer SYJ cannot effectively interact with graphene, has little effect on the aggregation state of graphene, and cannot change the dispersion state of graphene, so there is no obvious viscosity reduction effect. Although the viscosity and fluidity in Comparative Example 3 are acceptable, because the powder with low specific surface area, low oil absorption value and low conductivity is used, the pole sheet resistivity of Comparative Example 1 is very high (143Ω.cm) compared with the pole sheet resistivity of Example 1 of 3.81Ω.cm, and the conductivity is very poor.

[0183] Compared with Example 1, in Comparative Examples 4, 5 and 6, the viscosity reducer SYJ was replaced with ethanolamine, polyether TC109, and ethanolamine plus polyether TC109, and the other components were the same. As a result, the viscosity did not change significantly, which further illustrates the excellent viscosity reduction effect of SYJ, which cannot be achieved by any other additives.

[0184] Compared with Example 1, in Comparative Example 7, the solvent was changed to NMP, and the other components were the same. After grinding, the viscosity was very high and the fluidity was poor. After adding the viscosity reducer SYJ, the viscosity was also greatly reduced and the fluidity was improved, indicating that in the NMP system, the viscosity reducer SYJ also has a good viscosity reducing effect.

[0185] In summary, the viscosity reducer SYJ has an excellent viscosity reducing effect on graphene with high specific surface area, high oil absorption value, good conductivity and high defectivity (Id / Ig), and the process order has a great influence on the slurry viscosity. High-speed grinding and high shear force will cause the viscosity reducer SYJ to fail. Therefore, it is necessary to add the viscosity reducer after the slurry is ground. The viscosity reducing effect can be achieved by low-speed grinding or low-shear uniform dispersion. It is not limited to deionized water, but can also be applied to other solvents such as N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), etc.

[0186] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been presented as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A graphene slurry with high oil absorption value and low viscosity, characterized in that: Includes pre-dispersion and viscosity reducer; Wherein, the pre-dispersion liquid comprises graphene, a dispersant and a solvent; Calculated by mass percentage, the graphene slurry includes the following components: Graphene 0.5-6%, dispersant 0.5-3%, viscosity reducer 0.05-2%, and the balance is solvent; The viscosity reducer comprises a diamine group, a PPO group and a PEO group, and the diamine group is grafted with the PPO group or the PEO group.

2. The high oil absorption and low viscosity graphene slurry according to claim 1, characterized in that: The general structural formula of the viscosity reducer is as follows: Wherein, R contains a PPO group and a PEO group, and the value range of n is a positive integer between 1 and 20.

3. A graphene slurry with high oil absorption and low viscosity according to claim 1 or 2, characterized in that: The defect degree I of the graphene is determined according to the intensity ratio Id / Ig of the D peak and the G peak of the Raman spectrum, and the value range of the defect degree I is 0.8 to 1.

5.

4. The high oil absorption and low viscosity graphene slurry according to claim 3, characterized in that: The amount of the viscosity reducer added is calculated according to the following formula: Wherein, I is the defect degree of graphene, which is determined by the intensity ratio of D peak to G peak of Raman spectrum, Id / Ig, and the unit is 1; S is the mass percentage of graphene in the graphene slurry, in %; M is the mass percentage of the viscosity reducer in the graphene slurry, in %; B is the adjustment constant, the unit is 1, and the value range is 8≤B≤40.

5. The high oil absorption and low viscosity graphene slurry according to claim 1, characterized in that: The graphene is redox modified.

6. The high oil absorption and low viscosity graphene slurry according to claim 1, characterized in that: The graphene meets the following conditions: particle size distribution, D50≤100μm; specific surface area≥400m 2 / g; oil absorption value ≥2000ml / 100g.

7. The method for preparing a graphene slurry with high oil absorption and low viscosity according to claims 1 to 6, characterized in that: The steps include: Stirring and pre-dispersing graphene, a dispersant and a solvent to obtain a pre-dispersed liquid; Under the first parameter condition, grinding or shearing the pre-dispersed liquid to obtain an initial slurry; A viscosity reducing agent is added to the initial slurry, and the slurry is ground or sheared under the second parameter condition to obtain the graphene slurry with a set viscosity and particle size.

8. The method for preparing a graphene slurry with high oil absorption and low viscosity according to claim 7, characterized in that: The first parameter conditions include a rotation speed of 300 to 1000 rpm and a pump pressure of 0.1 to 0.3 bar.

9. The method for preparing a graphene slurry with high oil absorption and low viscosity according to claim 7, characterized in that: The second parameter conditions include a rotation speed of 50 to 400 rpm and a pump pressure of 0.1 to 0.3 bar.

10. The method for preparing a graphene slurry with high oil absorption and low viscosity according to claim 7, characterized in that: The set viscosity is ≤2000mPa.s at 10 inverse seconds; the set particle size D50 is 1-5um.