Degradable developing material and preparation process thereof
By using a combination of degradable polymer substances and developers in bone repair and soft tissue repair materials, the problem of poor development performance and difficulty in degradation of existing materials under X-rays is solved, achieving both the developability and mechanical properties of the material. , and improves its degradability, suitable for bone repair and soft tissue repair.
Patent Information
- Application Number
- CN202410886329.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
Existing bone repair and soft tissue repair materials have poor imaging performance under X-rays and are not easily degraded, making clinical application and evaluation difficult, and metal materials may cause osteoporosis.
It uses a combination of degradable polymer substances, developers and healing and repair substances, and combines polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer with α-tricalcium phosphate and corn starch, combined with polylactic acid-polymer Ethylene glycol nanocomposites are used as developers to prepare degradable developing materials with good mechanical properties and developability.
The material has both developability and degradability, and has good flexural strength, flexural modulus and compressive strength. It is still developed after one year, and the degradation rate reaches 83.2-89.5%, making it suitable for bone repair and soft tissue repair.
Smart Images

Figure BDA0004926152460000051 
Figure BDA0004926152460000052 
Figure BDA0004926152460000061
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of biomedical materials, and in particular to a degradable developing material and a preparation process thereof. Background Art
[0002] In recent years, with the continuous development of medical technology, bone repair, soft tissue repair and reconstruction materials have gradually become a hot topic in medical implant material research, and have been widely used in trauma, tumor, spinal orthopedic surgery, thoracic surgery and other fields.
[0003] At present, bone repair, soft tissue repair and reconstruction materials can be roughly divided into two categories: metal materials and non-metal materials. As for metal materials, their elastic modulus is relatively large, far exceeding that of human bones, and they are prone to stress shielding, thus causing osteoporosis or even degeneration, and metal materials are not easy to degrade. The raw materials used in non-metal materials are mostly low-density substances composed of carbon, hydrogen, and oxygen, and their imaging performance under X-rays is poor, which has caused great difficulties in clinical application and clinical evaluation. Therefore, it is urgent to develop a degradable imaging material. Summary of the invention
[0004] In order to improve the degradability of the material while maintaining the developing performance of the material, the present application provides a degradable developing material and a preparation process thereof.
[0005] In a first aspect, the present application provides a degradable developing material, which adopts the following technical solution: A degradable developing material comprises the following raw materials in parts by weight: 80-120 parts of a degradable high molecular substance, 1-5 parts of a developing agent, and 10-30 parts of a healing and repairing substance.
[0006] By adopting the above technical scheme, the degradable developing material of the present application can not only maintain the mechanical properties of the material, so that it has good bending strength, bending modulus and compressive strength, and has excellent developability, but also improve the degradability of the material, wherein the bending strength is 134-139MPa, the bending modulus is 7.0-7.7GPa, and the compressive strength is 62.0-62.5MPa. It still has obvious developability after one year, and the degradation rate of 28d is 12.1-15.8%, the degradation rate of 84d is 43.5-45.6%, and the degradation rate of 168d is 83.2-89.5%.
[0007] Degradable polymers are the basic components and the main raw materials of the developing materials. They have degradable properties and can improve the degradability of the developing materials. The developer is a drug that turns the latent image produced by the photosensitive material after exposure into a visible image. It can show the part to be repaired under X-rays, which is convenient for bone repair or soft tissue repair and clinical evaluation and application. Healing and repair substances are added to the raw materials of the degradable developing materials to promote the healing and repair of bones or soft tissues.
[0008] Preferably, the degradable polymer is a mixture of polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and a complex, and the weight ratio of polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and the complex is 1:1:1:1; wherein the complex is a compound of α-tricalcium phosphate and corn starch.
[0009] By adopting the above technical scheme, polylactic acid, polycaprolactone, and polylactic acid-glycolic acid copolymer are all degradable substances, and the composite is compounded with α-tricalcium phosphate and corn starch, wherein α-tricalcium phosphate is similar to the bone composition of the human body and can improve the bone repair ability, and α-tricalcium phosphate is extremely easy to degrade; corn starch is a natural polymer material with high biocompatibility and easy to obtain, and when corn starch meets water, it can gelatinize to form a grid structure and fully bond with α-tricalcium phosphate to improve the binding force between the composite particles, thereby improving the bone repair ability, and corn starch is also extremely easy to degrade, and after compounding with α-tricalcium phosphate, the formed composite can not only improve the bone repair ability, but also improve the degradability of the material.
[0010] Preferably, the healing and repairing substance is one or more of carboxymethyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, alginate, chitosan lactate, chitosan quaternary ammonium salt, and silk protein.
[0011] By adopting the above technical solution, the healing and repairing substances are limited, which facilitates better repair of bones or soft tissues.
[0012] Preferably, the composite is prepared by the following method: α-tricalcium phosphate and dibasic calcium phosphate dihydrate are placed in anhydrous ethanol, ball-milled, mixed evenly, dried, sieved to obtain substance A, substance A is mixed with corn starch, water is added, mixed evenly, and dried to obtain the composite.
[0013] Furthermore, the composite is prepared by the following method: α-tricalcium phosphate and dihydrate calcium hydrogen phosphate are placed in anhydrous ethanol, ball-milled for 2-4 hours, mixed evenly, dried, and passed through an 80-120 mesh sieve to obtain substance A; substance A is mixed with corn starch, water is added, mixed evenly, and dried to obtain a composite; The weight ratio of α-tricalcium phosphate to dihydrate calcium hydrogen phosphate is 1:(0.6-0.8), the amount of anhydrous ethanol added to each gram of α-tricalcium phosphate is 2-4 mL, and the amount of water added to each gram of α-tricalcium phosphate is 1-3 mL.
[0014] By adopting the above technical scheme and utilizing the above preparation method, the composite is prepared. First, α-tricalcium phosphate and dihydrate calcium hydrogen phosphate are dissolved, and then compounded with corn starch. When corn starch meets water, it will gelatinize, thereby enhancing the binding force with substance A. This not only improves the binding force between the composite and the part to be repaired, but also makes α-tricalcium phosphate and corn starch extremely easy to degrade, thereby further improving the degradability of the repair material.
[0015] Preferably, the weight ratio of α-tricalcium phosphate to corn starch is 1:(0.2-0.4).
[0016] If the amount of corn starch added is too little, it cannot be optimally compounded with α-tricalcium phosphate, and the degradability of the complex cannot be optimally improved, so the degradability of the repair material cannot be optimally improved; if the amount of corn starch added is too much, it will cause serious gelatinization, resulting in corn starch agglomeration, which is not easy to disperse, and cannot be optimally compounded with α-tricalcium phosphate, which will not only cause waste of corn starch, but also fail to optimally improve the degradability of the material. By adopting the above technical solution, when the weight ratio of α-tricalcium phosphate and corn starch is within the above range, not only will it not cause waste of corn starch, but it can also improve the degradability of the material.
[0017] Preferably, the developer is a polylactic acid-polyethylene glycol nanocomposite.
[0018] By adopting the above technical scheme, polylactic acid has good biodegradability and good biocompatibility, is non-toxic, non-irritating, has excellent mechanical properties, and is easy to form and process. However, polylactic acid cannot be developed under X-rays. By compounding polylactic acid and polyethylene glycol, polyethylene glycol has the effect of developing activation. The developer synthesized by the two is not only biodegradable, but also can improve the developing effect.
[0019] Preferably, the polylactic acid-polyethylene glycol nanocomposite is prepared by the following method: heating lactic acid and decompressing and dehydrating to obtain polylactic acid, adding polyethylene glycol, a catalyst, and a chain extender to the polylactic acid, and continuing to heat and heat to obtain a copolymer, adding dichloromethane to the copolymer, mixing evenly, adding anhydrous ethanol and water, mixing evenly, and stirring until the solvent evaporates to obtain a polylactic acid-polyethylene glycol nanocomposite.
[0020] Furthermore, the polylactic acid-polyethylene glycol nanocomposite is prepared by the following method: heating lactic acid to 80-100° C., decompressing and dehydrating to obtain polylactic acid, adding polyethylene glycol, a catalyst, and a chain extender to the polylactic acid, and continuing to heat to 140-170° C. to obtain a copolymer, adding dichloromethane to the copolymer, mixing evenly, adding anhydrous ethanol and water, mixing evenly, and stirring until the solvent evaporates to obtain a polylactic acid-polyethylene glycol nanocomposite; The weight ratio of lactic acid to polyethylene glycol is (6-10):1, the weight ratio of lactic acid to catalyst is 1:(0.4-0.6), the weight ratio of lactic acid to chain extender is 1:(0.1-0.2), the amount of dichloromethane added to each gram of lactic acid is 3-5 mL, the amount of anhydrous ethanol added to each gram of lactic acid is 7-9 mL, and the amount of water added to each gram of lactic acid is 7-9 mL.
[0021] By adopting the above technical solution and utilizing the above preparation method to prepare the polylactic acid-polyethylene glycol nanocomposite, it is convenient to prepare a degradable developer and to improve the developing effect of the material.
[0022] In a second aspect, the present application provides a process for preparing a degradable developing material, which adopts the following technical solution: A process for preparing a degradable developing material comprises the following steps: The polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and the composite are mixed evenly to obtain a degradable polymer; the degradable polymer, the healing and repairing substance and the developer are mixed evenly, melted, extruded and granulated to obtain a degradable developing material.
[0023] Preferably, the melting temperature is 60-80°C and the melting time is 20-30 minutes.
[0024] By adopting the above technical solution and utilizing the above preparation process to prepare the developing material, it is convenient to mix the various raw materials more evenly, and it is convenient to improve the degradability of the repair material while maintaining a good developing effect of the repair material.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. Since the composite material is formed by compounding α-tricalcium phosphate and corn starch in the present application, α-tricalcium phosphate is similar to the bone composition of the human body and can improve the bone repair ability, and α-tricalcium phosphate is extremely easy to degrade; corn starch is a natural polymer material with high biocompatibility and easy to obtain. When corn starch meets water, it can gelatinize to form a grid structure and fully adhere to α-tricalcium phosphate to improve the binding force between the composite particles, thereby improving the bone repair ability. Corn starch is also extremely easy to degrade. After compounding with α-tricalcium phosphate, the formed composite material can not only improve the bone repair ability, but also improve the degradability of the material, which can make the bending strength reach 139MPa, the bending modulus reach 7.7GPa, and the compressive strength reach 62.5MPa. It still has obvious developability after one year, and the degradation rate of 28d reaches 15.8%, the degradation rate of 84d reaches 45.6%, and the degradation rate of 168d reaches 89.5%.
[0026] 2. In this application, polylactic acid-polyethylene glycol nanocomposite is preferably used as the developer. Polylactic acid has good biodegradability and good biocompatibility, is non-toxic, non-irritating, has excellent mechanical properties, and is easy to form and process. However, polylactic acid cannot be developed under X-rays. Polylactic acid and polyethylene glycol are compounded. Polyethylene glycol has the effect of developing activation. The developer synthesized by the two is not only biodegradable, but also can improve the developing effect. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with the specific contents.
[0028] raw material The molecular weight of polylactic acid is 150,000; the molecular weight of polycaprolactone is 150,000; the molecular weight of polylactic acid-glycolic acid copolymer is 10,000; the healing and repairing substance is silk protein; the molecular weight of polyethylene glycol is 600; the catalyst is stannous octoate; and the chain extender is 1,6-hexamethylene diisocyanate.
[0029] Preparation Example Preparation Example 1 A composite is prepared by the following method: 2 kg of α-tricalcium phosphate and 1.4 kg of calcium hydrogen phosphate dihydrate were placed in 6 L of anhydrous ethanol, ball-milled for 3 h, mixed evenly, dried, and passed through a 100-mesh sieve to obtain substance A; substance A was mixed with 0.4 kg of corn starch, 4 L of water was added, mixed evenly, and dried to obtain a composite.
[0030] Preparation Example 2 A composite, which is different from Preparation Example 1 in that the amount of corn starch added is different, and the amount of corn starch added in Preparation Example 2 is 0.6 kg.
[0031] Preparation Example 3 A composite, which is different from Preparation Example 1 in that the amount of corn starch added is different, and the amount of corn starch added in Preparation Example 3 is 0.8 kg.
[0032] Preparation Example 4 A developer is prepared by the following method: 8 kg of lactic acid was heated to 90°C and dehydrated under reduced pressure to obtain polylactic acid. 1 kg of polyethylene glycol, 4 kg of catalyst and 1.2 kg of chain extender were added to the polylactic acid, and the temperature was continued to be raised to 155°C to obtain a copolymer. 32 L of dichloromethane was added to the copolymer and mixed evenly. 64 L of anhydrous ethanol and 64 L of water were added and mixed evenly. The mixture was stirred until the solvent evaporated to obtain a polylactic acid-polyethylene glycol nanocomposite. Example
[0033] Example 1 A degradable developing material, the raw material ratio of which is shown in Table 1.
[0034] A process for preparing a degradable developing material comprises the following steps: Polylactic acid, polycaprolactone, polylactic acid-hydroxyacetic acid copolymer, and the composite prepared in Preparation Example 1 are mixed evenly to obtain a degradable polymer; the degradable polymer, the healing and repairing substance, and the developer prepared in Preparation Example 4 are mixed evenly, melted at a temperature of 70°C for 25 minutes, extruded, and granulated to obtain a degradable developing material.
[0035] Example 2-3 A degradable developing material, which is different from Example 1 in that the raw material ratio of the developing material is different. The raw material ratio is shown in Table 1.
[0036] Table 1 Raw materials of developing materials in different embodiments Embodiment 4-5 A degradable developing material, which is different from Example 3 in that the raw material ratio of the developing material is different. The raw material ratio is shown in Table 2.
[0037] Table 2 Raw materials of developing materials in different embodiments Example 6 A degradable developing material, which differs from Example 4 in that the composite in the developing material raw material is prepared using Preparation Example 2.
[0038] Example 7 A degradable developing material, which differs from Example 4 in that the composite in the developing material raw material is prepared by Preparation Example 3.
[0039] Comparative Example Comparative Example 1 A degradable developing material, which differs from Example 1 in that an equal amount of the composite in the developing material raw material is replaced by polylactic acid.
[0040] Comparative Example 2 A degradable developing material, which differs from Example 1 in that an equal amount of the compound in the developing material raw material is replaced by α-tricalcium phosphate.
[0041] Performance testing The following performance tests were performed on the developer materials in Examples 1-7 and Comparative Examples 1-2: Bending strength, bending modulus, and compressive strength: The bending strength, bending modulus, and compressive strength of the developing material were measured using a bending elastic modulus tester and a compressive strength tester using a three-point load method. The test results are shown in Table 3.
[0042] Degradation rate: Take 1g of the developing material and dry it at 100℃ to constant weight. After measuring the constant weight, record it as m1. Add it to 150mL of normal saline, seal it, and let it stand in a constant temperature box at 37℃. Take out the sample at the set time, filter it, and weigh the filter residue (100℃). After measuring the constant weight, the weight of the filter residue is recorded as m2. The degradation rate is (m1-m2) / m1. The test results are shown in Table 4.
[0043] Development: The development material was implanted into the animal body and detected by X-ray. The material was observed after 12 months. The test results are shown in Table 4.
[0044] Table 3 Test results Table 4 Test results It can be seen from Table 3 and Table 4 that the degradable developing material of the present application can not only maintain the mechanical properties of the material, so that it has good bending strength, bending modulus and compressive strength, and has excellent developability, but also improve the degradability of the material, wherein the bending strength is 134-139 MPa, the bending modulus is 7.0-7.7 GPa, and the compressive strength is 62.0-62.5 MPa. It still has obvious developability after one year, and the degradation rate of 28 days is 12.1-15.8%, the degradation rate of 84 days is 43.5-45.6%, and the degradation rate of 168 days is 83.2-89.5%.
[0045] Combining Example 1 and Comparative Examples 1-2, it can be seen that the developing material in Example 1 has a bending strength of 134 MPa, a bending modulus of 7.0 GPa, and a compressive strength of 62.0 MPa. It still has obvious developability after one year. The degradation rate at 28 days is 12.1%, the degradation rate at 84 days is 43.5%, and the degradation rate at 168 days is 83.2%, which is better than Comparative Examples 1-2, indicating that it is more appropriate to add a composite to the material. The composite is a compound of α-tricalcium phosphate and corn starch, wherein α-tricalcium phosphate is extremely easy to degrade; corn starch is a natural polymer material with high biocompatibility and easy to obtain. When corn starch meets water, it can be gelatinized to form a grid structure and fully bonded with α-tricalcium phosphate to improve the binding force between the composite particles, thereby improving the bone repair ability. Corn starch is also very easy to degrade. After compounding with α-tricalcium phosphate, the formed composite can not only enable the material to maintain good mechanical properties and better developability, but also improve the degradability of the material.
[0046] In combination with Examples 1-3, it can be seen that the developing material in Example 3 has a bending strength of 135 MPa, a bending modulus of 7.2 GPa, and a compressive strength of 62.0 MPa. It still has obvious developability after one year, and the degradation rate at 28 days is 14.2%, the degradation rate at 84 days is 44.7%, and the degradation rate at 168 days is 87.4%, which is better than other examples, indicating that the addition amount of the composite in Example 3 is more appropriate, which can not only enable the material to maintain good mechanical properties and better developability, but also improve the degradability of the material.
[0047] Combining Example 4 with Examples 6-7, it can be seen that the developing material in Example 6 has a bending strength of 139 MPa, a bending modulus of 7.7 GPa, and a compressive strength of 62.3 MPa. It still has obvious developability after one year, and the degradation rate at 28 days is 15.8%, the degradation rate at 84 days is 45.6%, and the degradation rate at 168 days is 89.5%, which is better than other examples, indicating that the composite prepared by Preparation Example 2 is more suitable, which can not only enable the material to maintain good mechanical properties and better developability, but also improve the degradability of the material.
[0048] The above-mentioned specific implementation examples are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A degradable developing material, characterized in that: The invention comprises the following raw materials in parts by weight: 80-120 parts of degradable high molecular substances, 1-5 parts of developing agents and 10-30 parts of healing and repairing substances.
2. The degradable developing material according to claim 1, characterized in that: The degradable polymer substance is a mixture of polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and a composite, and the weight ratio of polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and the composite is 1:1:1:1; wherein the composite is compounded of α-tricalcium phosphate and corn starch.
3. The degradable developing material according to claim 1, characterized in that: The healing and repairing substance is one or more of carboxymethyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, alginate, chitosan lactate, chitosan quaternary ammonium salt, and silk protein.
4. The degradable developing material according to claim 2, characterized in that: The composite is prepared by the following method: α-tricalcium phosphate and dihydrate calcium hydrogen phosphate are put into anhydrous ethanol, ball-milled, mixed evenly, dried, sieved to obtain substance A, substance A is mixed with corn starch, water is added, mixed evenly, and dried to obtain the composite.
5. The degradable developing material according to claim 4, characterized in that: The weight ratio of α-tricalcium phosphate to corn starch is 1:(0.2-0.4).
6. The degradable developing material according to claim 1, characterized in that: The developer is a polylactic acid-polyethylene glycol nanocomposite.
7. The degradable developing material according to claim 6, characterized in that: The polylactic acid-polyethylene glycol nanocomposite is prepared by the following method: heating lactic acid to raise its temperature, decompressing and dehydrating to obtain polylactic acid, adding polyethylene glycol, a catalyst and a chain extender to the polylactic acid, continuing to heat and raise its temperature to obtain a copolymer, adding dichloromethane to the copolymer, mixing evenly, adding anhydrous ethanol and water, mixing evenly, and stirring until the solvent evaporates to obtain the polylactic acid-polyethylene glycol nanocomposite.
8. A process for preparing a degradable developing material according to any one of claims 1 to 7, characterized in that: The steps include: The polylactic acid, polycaprolactone, polylactic acid-glycolic acid copolymer and the composite are mixed evenly to obtain a degradable polymer; the degradable polymer, the healing and repairing substance and the developer are mixed evenly, melted, extruded and granulated to obtain a degradable developing material.
9. The process for preparing a degradable developing material according to claim 8, characterized in that: The melting temperature is 60-80°C and the melting time is 20-30 minutes.