Catalyst for catalytic oxidation of dichloromethane and acetone mixture and preparation method thereof
The spinel-type MnCr2Ox catalyst is prepared by the sol-gel method, which solves the low-temperature activity and stability problems in the catalytic oxidation of DCM and acetone mixtures in the existing technology, achieves high-efficiency catalytic oxidation, reduces pollution control costs, and provides A feasible solution for industrial VOCs treatment.
Patent Information
- Application Number
- CN202410892868.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for the existing technology to effectively catalyze the oxidation of dichloromethane (DCM) and acetone mixture in volatile organic compounds (VOCs), especially under low temperature conditions. The stability and activity of the catalyst are insufficient, resulting in high pollution control costs and harmful effects on human body and Environmental harm is great.
The spinel-type MnCr2Ox catalyst was prepared by the sol-gel method, and its excellent low-temperature oxidation activity and high-temperature stability were used to successfully catalyze the oxidation of a mixture of DCM and acetone, avoid the formation of polychlorine by-products, and maintain the stability during long-term reactions. active.
It achieves efficient catalytic oxidation of DCM and acetone at lower temperatures. The catalyst has no obvious deactivation within 24 hours. It has excellent durability and resistance to chlorine poisoning, reduces pollution control costs, and provides industrial multi-component VOCs. Possible ways to deal with it efficiently.
Smart Images

Figure HDA0004928119200000011 
Figure HDA0004928119200000021 
Figure HDA0004928119200000031
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nano material preparation, and relates to a catalyst for catalytic oxidation of a mixture of dichloromethane (DCM) and acetone and a preparation method thereof. Background Art
[0002] While the pharmaceutical industry brings economic growth and convenience to life, it also brings about a large amount of volatile organic compounds (VOCs) emissions. These pollutants have the problems of large total emissions, complex emission links, and high governance costs. For example, in the production of drugs such as cefaclor, amoxicillin and ampicillin, a large amount of DCM and acetone will be emitted at the same time. These gases will cause ozone layer destruction and induce smog weather when they are emitted into the atmosphere. Excessive inhalation of DCM and acetone will damage the human central nervous system and respiratory system, causing symptoms such as dizziness, headache, nausea, vomiting, chest tightness, and limb weakness, which is extremely harmful to the ecological environment and human health. Therefore, it is urgent to treat DCM and acetone waste gas. Catalytic oxidation has the characteristics of low reaction temperature and less secondary pollution. It is one of the most effective methods for removing VOCs. The key to this method is to develop a catalyst with good low-temperature oxidation activity, high-temperature stability and low price.
[0003] At present, the catalysts used for catalytic oxidation of VOCs are mainly divided into two categories: precious metals and transition metal oxide catalysts. Among them, oxides of transition metals such as Mn and Cr have good industrial application potential due to their low cost and high stability. They have variable oxidation states, better redox properties and higher active oxygen concentrations, and these physical and chemical properties can be controlled by changing the conditions during the material synthesis process, which is conducive to the rapid and deep oxidation of VOCs.
[0004] In this invention, we prepared a series of Mn-Cr composite oxide catalysts by sol-gel method and evaluated their catalytic oxidation performance on acetone and DCM mixture. x The catalyst can successfully catalyze the oxidation of DCM and acetone mixture at a relatively low temperature, has excellent durability, and has no obvious deactivation during the reaction process of up to 24 hours. To the best of our knowledge, there is no x The catalyst is reported to catalyze the oxidation of a mixture of DCM and acetone. Therefore, the present invention is innovative, and our research results are expected to provide a feasible method for the efficient treatment of industrial multi-component VOCs. Summary of the invention
[0005] The purpose of the present invention is to prepare a catalyst for catalytic oxidation of a mixture of DCM and acetone. A series of Mn-Cr composite oxides are prepared by a sol-gel method, wherein the prepared spinel MnCr2Ox The catalyst exhibited excellent activity and durability in the catalytic oxidation of DCM and acetone mixture.
[0006] A catalyst for catalytic oxidation of a mixture of DCM and acetone and a preparation method thereof, comprising the following steps:
[0007] Manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water, stirred at room temperature for 30 minutes, and then citric acid monohydrate was added. The solution was stirred in a water bath at 90°C until a viscous slurry was formed, and then the slurry was transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample; the molar ratio of manganese nitrate tetrahydrate to chromium nitrate nonahydrate was 1-2:1-2, preferably 1:2, and the amount of citric acid monohydrate was twice the molar amount of the metal nitrate. Further, according to the ratio of manganese nitrate tetrahydrate to chromium nitrate nonahydrate, different ratios of manganese chromium oxide Mn2CrO were obtained. x 、MnCrO x 、MnCr2O x .
[0008] Further Mn2CrO x Preparation of catalyst:
[0009] First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes. Then, citric acid monohydrate was added and the solution was stirred in a water bath at 90°C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate and citric acid monohydrate was 2:1:6.
[0010] Further MnCrO x Preparation of catalyst:
[0011] First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes, then citric acid monohydrate was added, and the solution was stirred in a water bath at 90°C until a viscous slurry was formed, and then the slurry was transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid, and finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate, and citric acid monohydrate was 1:1:4.
[0012] Further MnCr2O x Preparation of catalyst:
[0013] First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes, then citric acid monohydrate was added, and the solution was stirred in a water bath at 90°C until a viscous slurry was formed, and then the slurry was transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid, and finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate, and citric acid monohydrate was 1:2:6.
[0014] The catalyst obtained by the present invention is used for catalytic oxidation of a mixture of DCM and acetone. x The catalytic oxidation of DCM and acetone mixture was successful at a relatively low temperature, such as 240°C, with excellent durability and no obvious deactivation during the reaction process of up to 24 hours.
[0015] Catalyst Evaluation:
[0016] DCM and acetone were selected as the reaction gases for the evaluation of the relevant catalyst performance. The gas composition was 500ppm DCM+500ppm acetone+20vol% O2+N2 balance, and the space velocity (SV) was 20,000mL / (gh). x The catalyst not only has excellent activity but also has high selectivity for by-products, thus avoiding the generation of polychlorinated by-products during the catalytic reaction.
[0017] The catalyst of the invention has a simple preparation process, exhibits good catalytic activity for catalytic oxidation of a mixture of DCM and acetone, has strong resistance to chlorine poisoning, and has a long catalyst life, and has good application prospects in the field of air pollution control. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is the XRD pattern of the prepared catalyst.
[0019] Figure 2 MnCr2O x TEM, HRTEM, HAADF-STEM and elemental scanning images of the catalyst.
[0020] Where (A) is MnCr2O x TEM images of MnCr2O x HRTEM image of the catalyst, (D) is MnCr2O x HAADF-STEM image of the catalyst and elemental scanning images of Mn, Cr, and O.
[0021] Figure 3The curves of (A) acetone and (B) DCM conversion rates over the prepared catalysts during mixed VOCs oxidation at SV = 20,000 mL / (gh) as a function of temperature.
[0022] Figure 4 MnCr2O x Catalyst stability test diagram. DETAILED DESCRIPTION
[0023] To further illustrate the present invention, the following embodiments are described in detail, but the present invention is not limited to the following embodiments.
[0024] Example 1
[0025] (1) Preparation of Mn2O3 catalyst:
[0026] First, 60 mmol of manganese nitrate tetrahydrate was added to deionized water and stirred at room temperature for 30 min. Then, 120 mmol of citric acid monohydrate was added. The solution was stirred in a water bath at 90 °C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180 °C for 3 h to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace. The temperature was raised to 600 °C at a rate of 3 °C / min and calcined for 4 h to obtain the final sample.
[0027] (2) Mn2CrO x Preparation of catalyst:
[0028] First, 40 mmol of manganese nitrate tetrahydrate and 20 mmol of chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 min. Then, 120 mmol of citric acid monohydrate was added and the solution was stirred in a water bath at 90 °C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180 °C for 3 h to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600 °C at a rate of 3 °C / min and calcined for 4 h to obtain the final sample.
[0029] (3) MnCrO x Preparation of catalyst:
[0030] First, 30 mmol of manganese nitrate tetrahydrate and 30 mmol of chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 min. Then, 120 mmol of citric acid monohydrate was added and the solution was stirred in a water bath at 90 °C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180 °C for 3 h to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600 °C at a rate of 3 °C / min and calcined for 4 h to obtain the final sample.
[0031] (4) MnCr2O xPreparation of catalyst:
[0032] First, 20 mmol of manganese nitrate tetrahydrate and 40 mmol of chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 min. Then, 120 mmol of citric acid monohydrate was added and the solution was stirred in a water bath at 90 °C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180 °C for 3 h to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600 °C at a rate of 3 °C / min and calcined for 4 h to obtain the final sample.
[0033] (5) Preparation of Cr2O3 catalyst:
[0034] First, 60 mmol of chromium nitrate nonahydrate was added to deionized water and stirred at room temperature for 30 min. Then, 120 mmol of citric acid monohydrate was added and the solution was stirred in a water bath at 90 °C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180 °C for 3 h to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600 °C at a rate of 3 °C / min and calcined for 4 h to obtain the final sample.
[0035] (6) The prepared catalyst was used for catalytic oxidation of a mixture of DCM and acetone. 50 mg of the catalyst (particle size of 40-60 mesh) was weighed and loaded into a quartz fixed bed reactor. The mixed DCM and acetone reaction gas was introduced into the fixed bed reactor. The reaction gas composition was 500 ppm DCM + 500 ppm acetone, 20 vol% O2 and N2 (balance gas). The total gas flow rate was 16.7 mL / min and the SV was 20,000 mL / (gh). The reactor outlet gas was introduced into a gas chromatograph for online detection. It was found that as the reaction temperature increased, the detected DCM and acetone concentrations gradually decreased, and the MnCr2O x When catalyzing acetone and mixed gas, the conversion of acetone is T 50% and T 90% 150℃ and 182℃ respectively, and the T 50% and T 90% 215℃ and 250℃ respectively.
Claims
1. A method for preparing a catalyst for catalytic oxidation of a mixture of dichloromethane and acetone, characterized in that: The following steps are involved: Manganese nitrate tetrahydrate and chromium nitrate nonahydrate are added to deionized water, stirred at room temperature, and then citric acid monohydrate is added, and the solution is stirred in a water bath at 90°C until a viscous slurry is formed, and then the slurry is transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid. Finally, the solid is ground and placed in a muffle furnace, and the temperature is increased to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain a final sample; the molar ratio of manganese nitrate tetrahydrate to chromium nitrate nonahydrate is 1-2:1-2, preferably 1:2, and the amount of citric acid monohydrate is 2 times the molar amount of the metal nitrate.
2. The method for preparing a catalyst for catalytic oxidation of a mixture of dichloromethane and acetone according to claim 1, characterized in that: According to the ratio of manganese nitrate tetrahydrate and chromium nitrate nonahydrate, manganese chromium oxide Mn2CrO with different ratios can be obtained. x 、MnCrO x 、MnCr2O x .
3. The method for preparing a catalyst for catalytic oxidation of a mixture of dichloromethane and acetone according to claim 2, wherein Mn2CrO x Preparation of catalyst: First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes. Then, citric acid monohydrate was added and the solution was stirred in a water bath at 90°C until a viscous slurry was formed. The slurry was then transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid. Finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate and citric acid monohydrate was 2:1:
6.
4. The method for preparing a catalyst for catalytic oxidation of a mixture of dichloromethane and acetone according to claim 2, wherein MnCrO x Preparation of catalyst: First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes, then citric acid monohydrate was added, and the solution was stirred in a water bath at 90°C until a viscous slurry was formed, and then the slurry was transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid, and finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate, and citric acid monohydrate was 1:1:
4.
5. The method for preparing a catalyst for catalytic oxidation of a mixture of dichloromethane and acetone according to claim 2, wherein MnCr2O x Preparation of catalyst: First, manganese nitrate tetrahydrate and chromium nitrate nonahydrate were added to deionized water and stirred at room temperature for 30 minutes, then citric acid monohydrate was added, and the solution was stirred in a water bath at 90°C until a viscous slurry was formed, and then the slurry was transferred to an oven and heated at 180°C for 3 hours to obtain a fluffy solid, and finally, the solid was ground and placed in a muffle furnace, heated to 600°C at a rate of 3°C / min and calcined for 4 hours to obtain the final sample. The molar ratio of manganese nitrate tetrahydrate, chromium nitrate nonahydrate, and citric acid monohydrate was 1:2:
6.
6. The catalyst prepared by the method according to any one of claims 1 to 5.
7. Use of the catalyst prepared by the method according to any one of claims 1 to 5 for catalytic oxidation of a mixture of DCM and acetone.
8. The use according to claim 7, wherein the prepared MnCr2O x The catalytic oxidation of DCM and acetone mixture was successful at a relatively low temperature of 240°C, and there was no obvious deactivation during the reaction process of up to 24 hours.
Citation Information
Patent Citations
Preparation method and application of catalyst for catalytic oxidation of VOCs
CN106391009A
Double-perovskite composite metal oxide catalyst and preparation method and application thereof
CN106475105A
Method for preparing methyl cyclopentadiene under catalysis of AxByOz type composite metal oxide
CN114315504A
Application of non-noble metal cobalt-chromium alloy catalyst in catalytic combustion of low-carbon alkane
CN117000252A
Fluidizable catalyst for oxidative dehydrogenation of alkanes to olefins in an oxygen free environment
US20170233312A1