Heavy residual oil hydrodemetallization catalyst and preparation method thereof
By using a spherical cavity alumina carrier and hydrothermal treatment technology in the residual hydrodemetallization catalyst, an open pore structure is formed, which solves the problems of small surface pores and insufficient carbon deposition resistance of the existing catalyst, and achieves efficient removal of metal impurities and carbon deposit removal, improving the activity and stability of the catalyst.
Patent Information
- Application Number
- CN202310457453.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-26
AI Technical Summary
When existing residual oil hydrodemetallization catalysts treat heavy residual oil, the surface pores are small, making it difficult to effectively diffuse reactants, and the ability to resist carbon deposition is insufficient, making it difficult to completely remove metal impurities and residual carbon.
Using an alumina carrier containing spherical cavities, through a combination of micron spherical activated carbon and pseudo-boehmite, combined with hydrothermal treatment and propylene oxide sealing heat treatment, an open channel structure is formed, and flaky alumina grows on the surface and inside of the carrier Grains, improve the penetration and volume of the pore channel, enhance metal activity and anti-carbon deposition ability.
The pores on the surface of the catalyst are opened, the diffusion capacity and catalytic activity of the reactants are improved, the removal efficiency of metal impurities and carbon deposits is significantly improved, and the high activity and stability of the catalyst are ensured.
Smart Images

Figure CN118847136A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a heavy residue oil hydrodemetallization catalyst and a preparation method thereof. Background Art
[0002] Fixed bed residue oil hydrogenation process technology is mature and widely used. It is an effective means to achieve efficient conversion of heavy oil. Residue oil is enriched with most of the impurities such as sulfur, nitrogen, metals (mainly nickel and vanadium) in crude oil. Residue oil hydrogenation removes impurities such as metals, sulfur, nitrogen, etc. under high temperature and high pressure conditions through the action of catalysts, providing high-quality raw materials for downstream catalytic cracking. However, due to the high viscosity, high impurity content and complex molecular composition of residue oil, the hydrogenation reaction is difficult. It is difficult for a single catalyst to effectively remove impurities such as metals, sulfur, nitrogen and residual carbon in residue oil. At present, residue oil hydroprocessing catalysts usually include protective catalysts, demetallization catalysts, desulfurization catalysts and denitrification catalysts. Among them, the role of residue oil hydrogenation demetallization catalyst is to remove metals such as Ni and V in residue oil, and at the same time protect the desulfurization catalyst. It not only removes metal impurities in the feed, but also must accommodate as many of these metals and coke impurities as possible.
[0003] CN114425374A discloses a residual oil hydrodemetallization catalyst and a preparation method thereof, wherein the catalyst comprises a catalyst body composed of a carrier and an active component supported on the carrier, and a layer of carbon film is provided on the outer surface of the catalyst body. The carbon film covers the surface active center, so that during the residual oil hydrogenation process, the carbon deposits, sulfides, iron, calcium and other sediments generated after the residual oil reacts violently at the active sites on the catalyst surface are prevented from blocking the catalyst pores and covering the active sites, and the catalyst has good anti-coking performance. However, the surface pores of the hydrodemetallization catalyst prepared by the method are small, which is not conducive to the diffusion of residual oil reactant molecules into the catalyst interior.
[0004] CN104646008A discloses a catalyst for demetallization of inferior heavy oil by hydrodesulfurization and a preparation method thereof. The catalyst uses alumina as a carrier, and group VIII and VIB elements, especially Ni-Mo, as active components. The catalyst has a pore volume of 0.61-0.70 mL / g and a specific surface area of 155-200 m 2 / g, with an average pore diameter of 13.0-18.0nm. The catalyst preparation method is to treat the carrier particles after forming and calcining with an acid solution of continuously increasing concentration to improve the pore structure of the carrier and the hydrodemetallization catalyst. This method needs to be further improved in terms of increasing the macropore content of the alumina carrier, especially the effect of increasing the macropores on the surface.
[0005] CN110935461A discloses a method for preparing a heavy oil hydrogenation demetallization catalyst. The method for preparing the catalyst comprises: (1) kneading a physical pore expander, pseudo-boehmite and an active metal component, drying and calcining to obtain a modified alumina carrier SI; (2) spraying SI with an unsaturated impregnation solution I for the hydrogenation active component, and then drying and calcining to obtain a modified alumina carrier SII; (3) mixing SII, ammonium bicarbonate and water, and then performing a sealed heat treatment, and drying and calcining the material after the heat treatment to obtain a carrier SIII; (4) supersaturating the hydrogenation active component impregnation solution II for the carrier SIII, and then drying and calcining to obtain a catalyst. The surface of the catalyst prepared by this method has a rod-like structure, and the formed pores are open, which improves the catalyst's resistance to metal deposition and carbon deposition, but the rod-like alumina grown on the surface is easy to fall off, and the firmness of the bond with the main alumina needs to be further improved. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a heavy residue oil hydrodemetallization catalyst, wherein the hydrodemetallization catalyst has wide surface pores that are conducive to the diffusion of reactant molecules, has good internal pore permeability, and has strong metal impurity tolerance and carbon deposition resistance. The hydrodemetallization catalyst has high hydrodemetallization activity and activity stability, and is suitable for the field of heavy residue oil hydrodemetallization.
[0007] The heavy residue hydrodemetallization catalyst of the present invention comprises, based on the total weight of the catalyst, 80% to 90% of the alumina carrier containing spherical cavities, and MoO 3 The content is 9.5%-13.5%, the NiO content is 2.3%-3.3%, and the V 2 O 5 The content is 0.1%-0.8%, of which the percentage of the spherical cavity area in the cross section of the alumina carrier is 40%-60%; flake alumina grains are in-situ grown in the spherical cavity, the grain size is 100-600nm, and the volume proportion (filling rate) of the flake alumina in the spherical cavity is 40%-80%; the content of the hydrogenation active metals Mo, Ni, and V in the spherical cavity is calculated as MoO 3 The content is 13.0%-15.5%, the NiO content is 2.8%-4.5%, and the V 2 O 5 The content is 2.0%-3.5%; the outer surface of the alumina carrier is in-situ grown as flaky alumina grains, and the area ratio (coverage rate) of the flaky alumina on the outer surface is 85%-100%.
[0008] The preparation method of heavy residue oil hydrodemetallization of the present invention comprises the following contents: (1) impregnating micron-shaped spherical activated carbon with a first impregnation solution containing Mo, Ni, and V, and drying the impregnated activated carbon to obtain modified micron-shaped spherical activated carbon; (2) Mixing the modified micron spherical activated carbon, pseudo-boehmite and water to form a slurry, filtering and drying the slurry, kneading the dried material, drying and calcining the spherical pore-containing alumina carrier; (3) immersing the first alumina carrier in a propylene oxide aqueous solution for sealed heat treatment, separating the material from the solid and liquid after the treatment, and drying and calcining the solid phase material to obtain a second alumina carrier; (4) The second alumina carrier is impregnated with a second impregnation solution containing Mo and Ni. The impregnated material is dried and calcined to obtain a heavy residue oil hydrodemetallization catalyst.
[0009] In the method of the present invention, in the impregnation solution containing Mo, Ni and V in step (1), Mo is calculated as molybdenum oxide in an amount of 2.5-6.0 g / 100 mL, V is calculated as vanadium pentoxide in an amount of 1.2-2.4 g / 100 mL, and Ni is calculated as nickel oxide in an amount of 0.5-1.5 g / 100 mL. The amount of solution used is such that the micron-shaped spherical activated carbon is completely impregnated, and the impregnation time is 0.5-4 hours.
[0010] In the method of the present invention, the micron spherical activated carbon in step (1) has a diameter of 1-8 microns, and the micron spherical activated carbon can be prepared by existing methods or purchased. The drying temperature is 120-180° C. and the drying time is 4-10 hours.
[0011] In the method of the present invention, the mass ratio of the activated carbon modified with active metal to pseudo-boehmite in step (2) is 1:4-1:2, and the liquid-to-solid mass ratio of the slurry is 5:1-10:1.
[0012] In the method of the present invention, the kneading molding described in step (2) is carried out by conventional methods in the art, and an extrusion aid and a peptizing agent are added as needed during molding. The extrusion aid is sesbania powder, and the amount added is 0.1wt%-0.5wt% of the weight of the final alumina carrier. The peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the amount of the peptizing agent added is 0.1wt%-1.5wt% of the weight of the alumina carrier, which ultimately depends on the molding effect. The drying temperature is 100-160°C, and the drying time is 4-10 hours; the calcination temperature is 450-700°C, preferably 450-600°C, and the calcination time is 4-6 hours; the calcination is carried out in an oxygen-containing atmosphere.
[0013] In the method of the present invention, the mass percentage concentration of the propylene oxide aqueous solution in step (3) is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the first alumina carrier is 3:1-10:1, preferably 4:1-8:1.
[0014] In the method of the present invention, the sealed heat treatment in step (3) is preferably carried out in a closed autoclave, and the sealed heat treatment is preferably a two-step sealed heat treatment, i.e., firstly a low-temperature sealed heat treatment at 60-100°C for 1-4 hours, and then a sealed heat treatment at 110-180°C, preferably 120-160°C, for 14-20 hours.
[0015] In the method of the present invention, the drying temperature in step (3) is 100-160°C, the drying time is 2-8 hours, the roasting temperature is 500-750°C, the roasting time is 4-6 hours, and the roasting is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.
[0016] In the method of the present invention, in the second impregnation solution containing Mo and Ni in step (4), the Mo content is 8.5%-12.5 g / 100 mL as metal oxide, and the Ni content is 2.2-4.5 g / 100 mL as metal oxide.
[0017] In the method of the present invention, the drying temperature in step (4) is 100-160° C., the drying time is 2-8 hours, the roasting temperature is 450-550° C., and the roasting time is 4-6 hours.
[0018] The heavy residue oil hydrodemetallization catalyst of the present invention is used in the heavy residue oil hydrotreating process. The general reaction conditions are: reaction temperature 350-440°C, hydrogen oil volume ratio 500-1000, liquid hourly volume space velocity 0.5-1.5h -1 , operating pressure 12.5-15.5MPa.
[0019] Compared with the prior art, the present invention has the following advantages: The present invention first prepares an alumina carrier containing a large number of spherical cavities, wherein a certain amount of Mo, Ni, and V metals are directionally loaded in the spherical cavities, and then, through specific hydrothermal conditions and environments, flaky particles are in situ grown in the alumina cavities and outer surfaces, so that the carrier surface is accumulated to form open channels of 40-300nm. The channel structure is conducive to the diffusion of reactants, especially large-sized heavy residual oil reactants, into the catalyst, and a large number of 50-100nm channels with good penetration are formed in the spherical cavities, which are conducive to the diffusion of reactant molecules. At the same time, the hydrogenation active metal with high metal content is combined to improve the metal capacity, carbon deposition resistance, and metal support capacity of the spherical cavity, and the catalyst has high activity and activity stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the SEM image of the surface of the alumina carrier precursor prepared in Example 1.
[0021] Figure 2This is a cross-sectional SEM image of the alumina carrier precursor prepared in Example 1. Figure 3 This is the SEM image of the cross section of the alumina support prepared in Example 1. DETAILED DESCRIPTION
[0022] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.
[0023] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.
[0024] Bulk active metal content refers to the metal MoO in the overall catalyst. 3 The content of NiO was determined according to the method of ICP-AES determination of the content of metal elements in molybdenum-nickel series hydrogenation catalysts, Guangzhou Chemical Industry, 2021, 49, (17): 129-130.
[0025] The active metal content in the catalyst micro-area was determined using a scanning electron microscope equipped with an energy dispersive spectrometer (EDAX). During the determination, 20 micro-areas to be determined were randomly selected for composition determination and the average value was taken. The acceleration voltage was 30 KV and the working distance was 8 mm.
[0026] The active metal content in the micron-sized pores refers to the active metal content in the pores formed after the micron-sized activated carbon balls in the catalyst are calcined. During the measurement, the catalyst particles are cut and adhered to the sample stage of a scanning electron microscope so that the cross section of the catalyst particles is perpendicular to the direction of the electron beam of the scanning electron microscope. The scanning electron microscope is equipped with an energy spectrometer to determine the composition of this area.
[0027] Preparation of micron spherical activated carbon: The micron spherical activated carbon used in the method of the present invention is according to the literature: Dai Linlin, Li Wei, Wu Qiong, et al. Hydrothermal carbonization of carboxymethyl cellulose-CO 2 Preparation of micron-shaped spherical activated carbon by activation [J]. Chemistry and Industry of Forest Products, 2015, 35 (4): 21-27. The prepared micron-shaped spherical activated carbon has a diameter of 1-8 microns. Example 1
[0028] (1) Weigh 100 g of the above-mentioned micron-shaped spherical activated carbon and add molybdenum oxide at a concentration of 3.2 g / 100 mL. The material was impregnated with a molybdenum-nickel-vanadium solution having a nickel pentoxide concentration of 0.7 g / 100 mL and a vanadium pentoxide concentration of 2.1 g / 100 mL for 2 hours. The material was filtered after impregnation, and the spherical activated carbon was dried at 165°C for 5 hours to obtain active metal modified micron spherical activated carbon.
[0029] (2) Weigh 100 g of the active metal-modified micron spherical activated carbon and 275 g of pseudo-boehmite from step (1), add 6000 g of deionized water, and mechanically stir the mixture for 2 hours. After stirring, the material is separated into liquid and solid, and the solid material is dried at 120°C for 6 hours. Then, 2.0 g of sesbania powder is added to the dry material and mixed evenly. An appropriate amount of 0.5% acetic acid solution is kneaded evenly, and extruded into strips. The shaped material is dried at 130°C for 8 hours, and calcined at 550°C in an oxygen atmosphere for 5 hours to obtain an active metal-modified alumina carrier precursor S0. The surface scanning electron microscope image of the alumina carrier precursor is shown in FIG. Figure 1 , cross-sectional SEM images are shown in Figure 2 .
[0030] (3) Weigh 100 g of the active metal-modified alumina carrier precursor prepared in step (2), add 560 g of a 6.5% propylene oxide aqueous solution, transfer the mixture into an autoclave, seal the autoclave and place it in an oven, first seal it at 85° C. for 2.5 hours, then heat it to 150° C. and seal it for 17 hours. After cooling, wash and filter the material, dry the solid material at 120° C. for 6 hours, and calcine it at 650° C. for 5 hours to obtain an alumina carrier. The cross-sectional scanning electron micrograph of the carrier is shown in FIG. Figure 3 .
[0031] (4) Weigh 100 g of the alumina carrier prepared in step (3) and place it in a spray pot. Spray the alumina carrier with an active component impregnation solution having a molybdenum oxide concentration of 11 g / 100 mL and a nickel oxide concentration of 3.8 g / 100 mL in a saturated impregnation manner. The impregnated material is dried at 120° C. for 5 hours and calcined at 500° C. for 5 hours to obtain the hydrodemetallization catalyst Cat-1 of the present invention. The catalyst properties are shown in Table 1. Example 2
[0032] The same as Example 1, except that in step (1), the concentration of molybdenum oxide in the solution is 4.1 g / 100 mL, the concentration of nickel oxide is 0.9 g / 100 mL, and the concentration of vanadium pentoxide is 1.7 g / 100 mL; in step (2), the amount of pseudo-boehmite added is 300 g; in step (3), the concentration of propylene oxide is 5.4%, the amount of solution used is 620 g, and during hydrothermal treatment, it is first sealed and treated at 65° C. for 3.5 hours, and then the temperature is raised to 140° C. for 18.5 hours; in step (4), the concentration of molybdenum oxide in the active component impregnation solution is 10 g / 100 mL, and the concentration of nickel oxide is 2.5 g / 100 mL, to obtain the hydrodemetallization catalyst Cat-2 of the present invention, and the catalyst properties are shown in Table 1. Example 3
[0033] The same as Example 1, except that in step (1), the concentration of molybdenum oxide in the solution is 2.7 g / 100 mL, the concentration of nickel oxide is 0.6 g / 100 mL, and the concentration of vanadium pentoxide is 2.5 g / 100 mL; in step (2), the amount of pseudo-boehmite added is 250 g; in step (3), the concentration of propylene oxide is 7.5%, the amount of solution used is 450 g, and during hydrothermal treatment, it is first sealed and treated at 95° C. for 1.5 hours, then heated to 130° C., and the treatment time is 19.5 hours; in step (4), the concentration of molybdenum oxide in the active component impregnation solution is 11.5 g / 100 mL, and the concentration of nickel oxide is 3 g / 100 mL, to obtain the hydrodemetallization catalyst Cat-3 of the present invention, and the catalyst properties are shown in Table 1. Example 4
[0034] The same as Example 1, except that in step (1), the concentration of molybdenum oxide in the solution is 4.6 g / 100 mL, the concentration of nickel oxide is 1.0 g / 100 mL, and the concentration of vanadium pentoxide is 1.4 g / 100 mL; in step (2), the amount of pseudo-boehmite added is 350 g; in step (3), the concentration of propylene oxide is 4.3%, the amount of solution used is 760 g, and during hydrothermal treatment, it is first sealed and treated at 75° C. for 2 hours, then heated to 160° C., and the treatment time is 15.5 hours; in step (4), the concentration of molybdenum oxide in the active component impregnation solution is 9.5 g / 100 mL, and the concentration of nickel oxide is 2.3 g / 100 mL, to obtain the hydrodemetallization catalyst Cat-4 of the present invention, and the catalyst properties are shown in Table 1.
[0035] Comparative Example 1 The same method as in Example 1 was used, except that the aqueous solution of propylene oxide in step (3) was replaced with an aqueous solution of ammonia of the same mass concentration to obtain a comparative hydrodemetallization Cat-5. The catalyst properties are shown in Table 1.
[0036] Comparative Example 2 The same method as Example 1 was used, except that the aqueous propylene oxide solution in step (3) was replaced with an ethylene oxide solution of the same concentration to prepare a comparative hydrodemetallization catalyst Cat-6. The catalyst properties are shown in Table 1.
[0037] Comparative Example 3 The same method as Example 1, except that the concentration of propylene oxide in step (3) was 0.8%, was used to prepare a comparative hydrodemetallization catalyst Cat-7. The catalyst properties are shown in Table 1.
[0038] Comparative Example 4 The same as Example 1, except that in step (1), the micron spherical activated carbon was not modified with active metals, but the same amount of active metal solution was added during the carrier molding to obtain a comparative hydrogenation demetallization agent catalyst Cat-8. The catalyst properties are shown in Table 1.
[0039] Table 1 Catalyst properties
[0040] From the data in Table 1 and the accompanying drawings, it can be seen that the hydrodemetallization catalyst prepared by the method of the present invention has large pores on the surface, the pores are well opened, and the flaky particles accumulate in the micron-sized pores to form a large number of 50-100 nm pores. The active metal components in the micron-sized pores of the catalyst are Mo-Ni-V multiple components, and the content of active metal components in the micro-region is high. Example 5
[0041] The hydrodemetallization catalysts Cat-1 to Cat-4 prepared by the present invention and the hydrodemetallization catalysts Cat-5 to Cat-8 prepared by the comparative example were respectively loaded into a fixed bed hydrogenation reactor. The treated raw materials (see Table 2) were tested under the following conditions: reaction temperature 380°C, hydrogen-to-oil volume ratio 650, liquid hourly volume space velocity 1.0 h -1 , hydrogen partial pressure 15.0MPa, continuous operation 2000 hours, impurity removal properties are shown in Table 3.
[0042] Table 2 Raw oil properties
[0043] Table 3 Evaluation results of catalysts catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 Cat-8 Relative Ni removal rate, % 139 135 142 131 100 98 107 121 Relative V removal rate, % 137 134 136 128 100 106 111 125 It can be seen from the results in Table 3 that the hydrodemetallization catalyst prepared by the method of the present invention has a higher Ni and V removal rate and better activity stability.
Claims
1. A heavy residue hydrodemetallization catalyst, characterized in that: The percentage of the spherical cavity area in the cross section of the alumina carrier is 40%-60%; flaky alumina grains are in-situ grown in the spherical cavity, the grain size is 100-600nm, and the volume proportion of the flaky alumina in the spherical cavity is 40%-80%; the contents of the hydrogenation active metals Mo, Ni and V in the spherical cavity are 13.0%-15.5% MoO3, 2.8%-4.5% NiO and 2.0%-3.5% V2O5 on an oxide basis; the outer surface of the alumina carrier is in-situ grown as flaky alumina grains, and the area of the flaky alumina on the outer surface accounts for 85%-100%.
2. The catalyst according to claim 1, characterized in that: Based on the total weight of the catalyst, the content of the alumina carrier containing spherical cavities is 80%-90%, the content of MoO3 is 9.5%-13.5%, the content of NiO is 2.3%-3.3%, the content of V2O5 is 0.1%-0.8%, and the sum of the contents of each component is 100%.
3. A method for preparing heavy residue oil by hydrodemetallization according to claim 1 or 2, characterized in that The invention comprises the following contents: (1) impregnating micron-shaped spherical activated carbon with a first impregnation liquid containing Mo, Ni and V, and drying the impregnated activated carbon to obtain modified micron-shaped spherical activated carbon; (2) mixing the modified micron-shaped spherical activated carbon, pseudo-boehmite and water to form a slurry, filtering and drying the slurry, kneading the dried material, drying and calcining the slurry to obtain a first alumina carrier containing spherical pores; (3) immersing the first alumina carrier in an aqueous solution of propylene oxide for sealed heat treatment, separating the treated material from solid and liquid, and drying and calcining the solid phase material to obtain a second alumina carrier; (4) impregnating the second alumina carrier with a second impregnation liquid containing Mo and Ni, and drying and calcining the impregnated material to obtain a heavy residue oil hydrodemetallization catalyst.
4. The method according to claim 3, characterized in that: In the impregnation solution containing Mo, Ni and V in step (1), Mo is calculated as molybdenum oxide in an amount of 2.5-6.0 g / 100 mL, V is calculated as vanadium pentoxide in an amount of 1.2-2.4 g / 100 mL, and Ni is calculated as nickel oxide in an amount of 0.5-1.5 g / 100 mL. The amount of solution used is such that the micron-shaped spherical activated carbon is completely impregnated, and the impregnation time is 0.5-4 hours.
5. The method according to claim 3, characterized in that: The micron spherical activated carbon in step (1) has a diameter of 1-8 microns and is prepared by an existing method or purchased; the drying temperature is 120-180° C. and the drying time is 4-10 hours.
6. The method according to claim 3, characterized in that: The mass ratio of the activated carbon modified with active metal to pseudo-boehmite in step (2) is 1:4-1:2, and the liquid-solid mass ratio of the slurry is 5:1-10:
1.
7. The method according to claim 3, characterized in that: The mass percentage concentration of the propylene oxide aqueous solution in step (3) is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the first alumina carrier is 3:1-10:1, preferably 4:1-8:
1.
8. The method according to claim 3, characterized in that: The sealed heat treatment in step (3) is carried out in a closed autoclave, and the sealed heat treatment is preferably a two-step sealed heat treatment, i.e., first a low-temperature sealed heat treatment at 60-100°C for 1-4 hours, and then a sealed heat treatment at 110-180°C, preferably 120-160°C, for 14-20 hours.
9. The method according to claim 3, characterized in that: The drying temperature in step (3) is 100-160°C, and the drying time is 2-8 hours; the roasting temperature is 500-750°C, and the roasting time is 4-6 hours.
10. The method according to claim 3, characterized in that: In the second impregnation solution containing Mo and Ni in step (4), the Mo content is 8.5%-12.5 g / 100 mL as metal oxide, and the Ni content is 2.2-4.5 g / 100 mL as metal oxide.
11. The method according to claim 3, characterized in that: The drying temperature in step (4) is 100-160°C, the drying time is 2-8 hours, the roasting temperature is 450-550°C, and the roasting time is 4-6 hours.
12. Use of the heavy residue oil hydrodemetallization catalyst according to claim 1 or 2 in a heavy residue oil hydrotreating process, wherein the reaction conditions are: reaction temperature 350-440°C, hydrogen-oil volume ratio 500-1000, liquid hourly volume space velocity 0.5-1.5h -1 , operating pressure 12.5-15.5MPa.
Citation Information
Patent Citations
Method for preparing spherical aluminum oxide
CN103055950A
Preparation method of catalyst for propane oxidative dehydrogenation to propylene
CN105727980A
Dehydrogenation catalyst and preparation method thereof
CN108579742A
Alumina carrier, hydrodemetallization catalyst and preparation method of hydrodemetallization catalyst
CN111822012A
Mesoporous microsphere alumina carrier and preparation method thereof, and desulfurization and denitrification catalyst and preparation method thereof