Calcium-based CO2 adsorbent as well as preparation method and application thereof
Patent Information
- Application Number
- CN202310605028.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Calcium-based CO2 adsorbents have problems with insufficient wear resistance and stability during use, especially in motion process scenarios, sintering and channel collapse are prone to occur, resulting in reduced adsorption capacity and unstable structural structure.
Using a preparation method, by mixing silicon-containing compounds with solvents, adjusting pH, adding carbon sources and additives, heat treatment and microwave heating, a calcium-based CO2 adsorbent with high mechanical strength and chemical stability is formed, and carbon is used. The source acts as a template agent and a pore-forming agent to form a stable silicon carbide skeleton to prevent CaO from sintering.
The high wear resistance, sintering and high adsorption capacity of calcium-based CO2 adsorbent is achieved, ensuring the stability of long-term recycling and maintaining chemical stability in process scenarios where materials are mixed.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorption separation, and in particular relates to an adsorption material for carbon dioxide adsorption separation and a preparation method thereof. Background Art
[0002] High temperature solid CO 2 The adsorbent can be used to remove CO in flue gas or tail gas from coal-fired power plants or other industrial processes. 2 Direct capture, no need to cool the high temperature gas first, simple and easy, calcium-based CO 2 The adsorbent has become the most promising high-temperature solid CO adsorbent due to its fast adsorption rate and high theoretical capacity. 2 Adsorbent. At the same time, calcium-based CO 2 The adsorbent can also be used in other processes to capture CO in situ. 2 Or use it to adsorb and desorb CO 2 The process completes the process of CO 2 For example, in chemical processes such as biomass gasification, ethanol reforming hydrogen production, and methane hydrogen production, calcium-based CO 2 The application of adsorbents can affect the reaction balance, change the reaction path, and improve product quality. 2 Adsorbents often need to move in different reactors or even be directly mixed with materials, which places higher demands on their wear resistance and stability.
[0003] Since CaCO 3 The Taman temperature is low, CaCO 3 Due to the large difference in molar volume between calcium-based CO and CaO, 2 The adsorbent is regenerated by carbonation / calcination to complete the CO 2 During the adsorption and desorption cycle, the effective components are prone to sintering and fusion, and the pores are prone to collapse, causing the carbonation conversion rate of the adsorbent to decay rapidly, the adsorption capacity to decrease rapidly, and the specific surface area to decrease significantly. To address the above problems, researchers have mostly provided skeleton support, alleviated the sintering of the adsorbent, and maintained its structural characteristics by doping high-Taman temperature-inert components containing Zr and other materials and regulating the morphology. However, after the above modifications, the mechanical strength of the calcium-based adsorbent is limited. In process scenarios where the adsorbent needs to move, especially in moving bed and fluidized bed processes, its strength is far from meeting the requirements. At the same time, traditional high-Taman temperature-inert components are not very effective in adsorbing CO2 in the flue gas of coal-fired power plants. 2 It is relatively stable when mixed with other materials, but it may react in some process scenarios where it is mixed with other materials, thus affecting the stability of the calcium-based adsorbent.
[0004] CN102671618A discloses a microsphere nano-CaO-based CO 2Preparation method of adsorbent, nano CaCO 3 After the suspension, additives and aluminum sol are mixed evenly, microsphere particles are obtained by spray granulation, and then calcined to obtain the adsorbent. However, the adsorbent prepared by the above patent still has great wear and tear, and it is still difficult to use it in the process scenario of mixing with materials. Summary of the invention
[0005] For existing CO 2 The core purpose of the present invention is to provide a calcium-based CO 2 The invention relates to an adsorbent and a preparation method and application thereof. The preparation method is simple and easy, and the obtained adsorbent has the advantages of wear resistance, high adsorption capacity, sintering resistance, microwave heating, etc., and can be used in a long-term cycle.
[0006] The technical solution of the present invention mainly includes the following aspects:
[0007] The first aspect of the present invention provides a calcium-based CO 2 The preparation method of the adsorbent comprises the following steps:
[0008] (1) contacting and mixing a silicon-containing compound with a solvent A, and then adjusting the pH value of the system to obtain a material stream A;
[0009] (2) mixing feed stream A, additive A, and carbon source, and obtaining feed stream B after heat treatment;
[0010] (3) The material stream B, the calcium source, and the solvent B are mixed evenly, and then the additive B is introduced, and the material stream C is obtained after drying, and further treated under microwave conditions to obtain the calcium-based CO 2 Adsorbent.
[0011] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the silicon-containing compound in step (1) is selected from one or more of soluble silicates, alkoxysilanes, and silicon tetrachloride; more specifically, the soluble silicate can be one or more of sodium silicate, lithium silicate, potassium silicate, ammonium silicate, etc., and the alkoxysilane can be one or more of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate, dimethyldiethoxysilane, methyltriethoxysilane, methyltrimethoxysilane, vinyltriethoxysilane, n-octyltriethoxysilane, etc.; preferably one or more of sodium silicate, ethyl orthosilicate, and dimethyldiethoxysilane.
[0012] Preferably, the calcium-based CO 2In the preparation method of the adsorbent, the solvent A in step (1) is water or a mixture of water and organic solvents, the organic solvent is an alcohol, and the alcohol is selected from one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and is more preferably ethanol. When the solvent A is a mixture of water and alcohol, the concentration of the alcohol is 1wt% to 80wt%.
[0013] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the solvent A in step (1) also includes component A, wherein component A can be one or more of silicone oil, hexamethylenetetramine, formamide, N,N-dimethylformamide, and polyethylene glycol (molecular weight of 200-20000); calculated based on the weight of the silicon-containing compound, the content of component A is 1wt% to 50wt%.
[0014] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the pH value of the control system in step (1) is 1 to 12, preferably 1 to 10; the pH value of the system can be controlled by introducing an acid or ammonia water, and the acid can be one or more of nitric acid, hydrochloric acid, phosphoric acid, oxalic acid, and citric acid.
[0015] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the auxiliary agent A described in step (2) is one or more of metal nitrates, metal carbonates, metal phosphates, metal organic acid salts, and metal chlorides, wherein the corresponding metal cations in the salt can be selected from one or more of aluminum, iron, magnesium, copper, silver, nickel, zirconium, cerium, lanthanum, yttrium, manganese, titanium, ytterbium, and neodymium; preferably, the auxiliary agent A is selected from one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, zirconium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, manganese nitrate, titanium tetrachloride, ytterbium nitrate, neodymium nitrate, basic aluminum acetate, magnesium acetate, magnesium oxalate, zirconium acetate, etc., and more preferably, the auxiliary agent A is one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, and zirconium nitrate.
[0016] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the carbon source in step (2) can be one or more of activated carbon, carbon black, and semi-coke, preferably activated carbon, and more preferably the specific surface area of the activated carbon is greater than 200 m 2 / g; the activated carbon can be one or more of biomass-based activated carbon, coal-based activated carbon, and petroleum-based activated carbon, preferably biomass-based activated carbon. The carbon source can be selected from commercial products or prepared according to the methods disclosed in the prior art.
[0017] Preferably, the calcium-based CO 2In the method for preparing the adsorbent, the carbon source in step (2) can be prepared by the following method: the biomass and the activator are uniformly mixed, and then subjected to heat treatment and washing to obtain the carbon source.
[0018] Furthermore, the biomass may be one or more of wood chips, coconut shells, straw, bamboo chips, rice husks, tung oil shells, grapefruit peels, starch, lignin, and cellulose.
[0019] Furthermore, the activator may be one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, zinc chloride, phosphoric acid, and sulfuric acid.
[0020] Furthermore, the heat treatment temperature is 350-900° C., the heat treatment time is 0.5-10 hours, and the heat treatment is carried out in the presence of nitrogen or an inert gas, wherein the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0021] Furthermore, the washing is performed by washing with an acid solution or an alkaline solution and then washing with deionized water until no activator ions are detected. The acid can be one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid, and the alkali can be one or more of sodium hydroxide, potassium hydroxide, and lithium hydroxide.
[0022] Furthermore, the mass ratio of the activator to the biomass is 0.2:1 to 5:1.
[0023] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, based on the mass of the silicon-containing compound, the dry basis content of the auxiliary agent A is 0.01wt% to 10.0wt%, and the mass ratio of the carbon source to the silicon-containing compound is 0.1:1 to 10:1.
[0024] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the heat treatment in step (2) includes two steps of drying and calcining, wherein the drying temperature is 100-150°C, the calcining temperature is 350-900°C, the calcining time is 0.2-10 hours, and the calcining is carried out in the presence of a reducing atmosphere; the reducing atmosphere is any one of a reducing gas and a mixed gas of a reducing gas and an inert atmosphere; the reducing gas is one or more of hydrogen, carbon monoxide, methane, and C2-C4 gas, preferably hydrogen and / or methane; in the mixed gas, the volume content of the reducing gas is 0.5%-99.5%. The inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0025] Preferably, the calcium-based CO 2In the method for preparing the adsorbent, the carbon source in step (2) can be crushed and sieved as needed before mixing, and a carbon source with a mesh size of 10-80 is preferred.
[0026] Preferably, the calcium-based CO 2 In the method for preparing the adsorbent, in step (2), separation treatment is preferably performed before heat treatment, and the solid phase material obtained by separation is subjected to heat treatment.
[0027] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the calcium source in step (3) can be one or more of calcium oxide, calcium hydroxide, and calcium salt. Preferably, the calcium source is one or more of calcium oxide, calcium oxalate, calcium gluconate, calcium hydroxide, calcium carbonate, calcium acetate, calcium propionate, calcium acetylacetonate, calcium lactate, calcium formate, calcium citrate, and calcium nitrate. More preferably, the calcium source is one or more of calcium oxide, calcium oxalate, and calcium nitrate.
[0028] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the solvent B in step (3) is water and / or an organic solvent; the organic solvent is preferably an alcohol solvent, and the alcohol solvent is a small molecule (carbon atom number is 1-4) alcohol solvent, which can be specifically selected from one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and is more preferably ethanol; when solvent B is a mixed solvent of water and an organic solvent, the concentration of the organic solvent is 1wt% to 80wt%.
[0029] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the auxiliary agent B in step (3) can be selected from one or more of carboxymethyl cellulose, hydroxyethyl cellulose, microcrystalline cellulose, chitosan, sesbania powder, hydroxypropyl methyl cellulose, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol, aluminum dihydrogen phosphate and their solutions, preferably one or more of carboxymethyl cellulose, sesbania powder, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol and their solutions.
[0030] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, in step (3), based on the mass of the calcium source, the mass ratio of solvent B to the calcium source is 0.2:1 to 20:1, the mass ratio of stream B to the calcium source is 0.01:1 to 2:1, and the dry basis content of additive B is 0.5wt% to 10wt%.
[0031] Preferably, the calcium-based CO 2In the preparation method of the adsorbent, in step (3), a molding treatment is preferably performed before drying. The molding technology is an existing technology known to those skilled in the art. The specific molding operation can be selected by those skilled in the art according to actual needs. The shape can be any shape such as cylindrical strip, clover, four-leaf clover, sphere, etc., preferably sphere. The ball molding method can be one or more of extrusion ball molding, rolling molding, and spray drying molding.
[0032] Preferably, the calcium-based CO 2 In the method for preparing the adsorbent, the drying temperature in step (3) is 100-150°C.
[0033] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, after drying in step (3), a calcination treatment can be further performed, the calcination temperature is 350 to 900° C., the calcination time is 1 to 10 hours, and the calcination is performed under the condition of an inert atmosphere, wherein the inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0034] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the microwave power in step (3) is 10-1000 W / (g material), preferably 100-500 W / (g material); the microwave treatment time is 0.1 to 10 hours, preferably 0.1 to 1 hour; the microwave treatment is further preferably carried out in the presence of an inert gas, wherein the inert gas is one or more of helium, neon, argon, krypton and xenon.
[0035] Preferably, the calcium-based CO 2 In the preparation method of the adsorbent, the calcium-based CO 2 The preparation method of the adsorbent further comprises step (4), wherein the step (4) is to heat-treat the material obtained in step (3) under oxygen-containing atmosphere conditions, wherein the heat-treating temperature is 500-1300° C., preferably 500-800° C., and the heat-treating time is 0.5-8 hours. The oxygen-containing atmosphere can be any one of air, oxygen, and a mixed gas of oxygen and an inert atmosphere, wherein the volume content of oxygen in the mixed gas is 5-99.99%; the inert atmosphere is nitrogen and / or an inert gas, wherein the inert gas is one or more of helium, neon, argon, krypton, and xenon.
[0036] The second aspect of the present invention provides a calcium-based CO obtained by the above preparation method. 2 Adsorbent.
[0037] The third aspect of the present invention provides a calcium-based CO obtained by the above preparation method. 2 The adsorbent adsorbs CO 2Application in.
[0038] The calcium-based CO provided by the present invention 2 The technical effects and advantages of the adsorbent and its preparation method are mainly reflected in the following aspects:
[0039] 1. The calcium-based CO provided by the present invention 2 In the adsorbent preparation method, the carbon source plays the role of template and pore-forming agent to a certain extent. While generating the silicon carbide skeleton, it also guides the regulation of the adsorbent surface morphology, promotes the formation of pore structure, buffers the change of local volume during the adsorption and desorption cycle, ensures structural stability, and is beneficial to CO 2 diffusion and adsorption.
[0040] 2. The calcium-based CO provided by the present invention 2 In the adsorbent preparation method, additive A can form metal particles on the surface of the precursor particles, which interact strongly with microwaves to produce Joule heating effect, and even induce microwave discharge, causing local drastic temperature rise, and strengthening the microwave selective heating effect; secondly, the metal particles can also generate high Tamman temperature inert components that alleviate the sintering of CaO particles. At the same time, the introduction of metal active components (such as nickel, iron, and cobalt) can also reduce the difficulty of silicon carbide synthesis.
[0041] 3. The calcium-based CO provided by the present invention 2 In the adsorbent preparation method, the material is heated under microwave conditions. The huge differences in the dielectric properties of different components are utilized to form hot spots among carbon, metal particles and newly generated silicon carbide, thereby strengthening the hot spot effect and selective heating effect of microwaves, promoting the rapid generation of silicon carbide and the formation of a supporting skeleton, and preventing the sintering of CaO active particles, thereby solving the problem of in-situ generation of silicon carbide.
[0042] 4. The calcium-based CO provided by the present invention 2 In the adsorbent preparation method, silicon carbide with excellent mechanical strength and thermal stability is introduced through in-situ reaction as a supporting skeleton, which can effectively alleviate and prevent the sintering of CaO, thereby improving its wear resistance while ensuring the adsorption capacity and cycle stability. At the same time, the chemical inertness of silicon carbide can also ensure that the adsorbent maintains chemical stability in process scenarios such as direct mixing with materials, which is beneficial to the long-term recycling of the adsorbent. DETAILED DESCRIPTION
[0043] The specific contents and effects of the method of the present invention are further described below by way of specific examples, but the scope of the present invention is not limited thereby. In the present invention, the molecular weight of the polyvinyl alcohol is the viscosity average molecular weight.
[0044] The specific embodiments of the present invention are described in detail below, but it should be pointed out that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims in the appendix.
[0045] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definitions in this specification shall prevail.
[0046] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0047] Unless otherwise expressly indicated, throughout the specification and claims, the term "comprise" or its variations such as "include" or "comprising" etc. will be understood to include the stated elements or components without excluding other elements or other components. In this document, all numerical values of parameters (e.g., quantities or conditions) are to be understood as being modified in all cases by the term "about", regardless of whether "about" actually appears before the numerical value.
[0048] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.
[0049] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0050] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.
[0051] Example 1
[0052] After the bamboo charcoal powder and potassium hydroxide are evenly mixed, they are kept at a constant temperature for 4 hours at 800°C in a nitrogen atmosphere. The mass ratio of potassium hydroxide to bamboo charcoal powder is 0.8:1. After washing with hydrochloric acid solution, they are washed with deionized water to obtain a carbon source. N,N-dimethylformamide is added to deionized water containing 1% methanol, stirred rapidly, sodium silicate is slowly added, and the pH is adjusted to 1-2 with hydrochloric acid to obtain stream A. The carbon source and nickel nitrate are slowly added to stream A. Based on the mass of sodium silicate, the content of N,N-dimethylformamide is 50%, the content of nickel nitrate is 0.2%, and the mass ratio of carbon source to sodium silicate is 2:1. Dry at 150°C, and then keep the temperature at 900°C in a nitrogen atmosphere for 0.2 hours to obtain stream B.
[0053] Slowly add calcium oxide to deionized water containing 5% ethanol, stir quickly, then slowly add stream B, and then slowly add carboxymethyl cellulose and silica sol. Wherein, based on the mass of calcium oxide, the mass ratio of solvent to calcium oxide is 20:1, the weight ratio of stream B to calcium oxide is 1.5:1, the dry basis content of carboxymethyl cellulose is 5%, and the dry basis content of silica sol is 1%. The above materials are prepared into microspheres, dried at 150°C, and then kept at a constant temperature of 500°C in a nitrogen atmosphere for 5 hours. The above materials are sent to a microwave roasting furnace and treated at a power of 400W / (g material) for 1 hour in an argon atmosphere. The above materials are kept at a constant temperature of 850°C for 0.5 hours in a nitrogen atmosphere containing 5% oxygen to obtain calcium-based CO 2 Adsorbent.
[0054] Example 2
[0055] Potassium silicate was slowly added into deionized water, stirred rapidly, and the pH was adjusted to 2-3 with nitric acid to obtain stream A. Carbon black and magnesium nitrate were slowly added into stream A, with the content of magnesium nitrate being 2% based on the mass of potassium silicate, and the mass ratio of carbon black to potassium silicate being 5:1. Drying was performed at 120°C, and then the mixture was kept at a constant temperature of 900°C for 2 hours in an ethane atmosphere to obtain stream B.
[0056] Calcium lactate is slowly added to deionized water containing 80% butanol, stirred rapidly, and then stream B is slowly added, and then microcrystalline cellulose and aluminum dihydrogen phosphate are slowly added. Wherein, based on the mass of calcium lactate, the mass ratio of solvent to calcium lactate is 7:1, the weight ratio of stream B to calcium lactate is 0.5:1, the dry basis content of microcrystalline cellulose is 9%, and the dry basis content of aluminum dihydrogen phosphate is 1%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 800°C in a nitrogen atmosphere for 1 hour. The above materials are sent to a microwave roasting furnace and treated at a power of 1000W / (g material) for 0.5 hours in an argon atmosphere. The above materials are kept at a constant temperature of 450°C in an oxygen atmosphere for 8 hours to obtain calcium-based CO 2 Adsorbent.
[0057] Example 3
[0058] Hexamethylenetetramine was added to deionized water containing 50% propanol, stirred rapidly, ethyl orthosilicate was slowly added, and the pH was adjusted to 8-9 with aqueous ammonia to obtain stream A. Activated carbon (specific surface area of about 700 m 2 / g), nickel nitrate and zirconium nitrate are slowly added into feed stream A. Based on the mass of tetraethyl orthosilicate, the content of hexamethylenetetramine is 15%, the content of nickel nitrate is 0.15%, the content of zirconium nitrate is 9%, and the mass ratio of activated carbon to tetraethyl orthosilicate is 1:1. Dry at 120°C, and then keep the temperature at 350°C in a hydrogen atmosphere for 10 hours to obtain feed stream B.
[0059] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then stream B is slowly added, and then silica sol is slowly added. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 15:1, the weight ratio of stream B to calcium nitrate is 0.35:1, and the dry basis content of silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C for 2 hours in a nitrogen atmosphere. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 1 hour in an argon atmosphere. The above materials are kept at a constant temperature of 650°C in an air atmosphere for 1 hour to obtain calcium-based CO 2 Adsorbent.
[0060] Example 4
[0061] Add formamide to deionized water containing 70% ethanol, stir rapidly, slowly add propyl orthosilicate, and adjust the pH to 9-10 with aqueous ammonia to obtain stream A. Slowly add semi-coke and aluminum nitrate to stream A, based on the mass of propyl orthosilicate, the formamide content is 10%, the aluminum nitrate content is 5%, and the mass ratio of semi-coke to propyl orthosilicate is 0.3:1. Separate the solid and liquid, dry at 100°C, and then keep constant temperature at 750°C for 3 hours in a propane atmosphere to obtain stream B.
[0062] Calcium gluconate is slowly added to deionized water containing 10% glycerol, stirred rapidly, and then stream B is slowly added, and then sesbania powder and carboxymethyl cellulose are slowly added. Wherein, based on the mass of calcium gluconate, the mass ratio of solvent to calcium gluconate is 3:1, the weight ratio of stream B to calcium gluconate is 0.25:1, the dry basis content of sesbania powder is 5%, and the dry basis content of carboxymethyl cellulose is 5%. The above materials are prepared into microspheres and dried at 100°C. The above materials are sent to a microwave roasting furnace and treated at a power of 150W / (g material) for 3 hours in an argon atmosphere. The above materials are kept at a constant temperature of 600°C for 0.5 hours in a nitrogen atmosphere containing 75% oxygen to obtain calcium-based CO2 Adsorbent.
[0063] Comparative Example 1
[0064] Hexamethylenetetramine was added to deionized water containing 50% propanol, stirred rapidly, ethyl orthosilicate was slowly added, and the pH was adjusted to 8-9 with aqueous ammonia to obtain stream A. Activated carbon (specific surface area of about 700 m 2 / g) was slowly added into the feed stream A, based on the mass of tetraethyl orthosilicate, the content of hexamethylenetetramine was 15%, and the mass ratio of activated carbon to tetraethyl orthosilicate was 1:1. It was dried at 120°C and then kept at a constant temperature of 350°C in a hydrogen atmosphere for 10 hours to obtain a feed stream B.
[0065] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then stream B is slowly added, and then silica sol is slowly added. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 15:1, the weight ratio of stream B to calcium nitrate is 0.35:1, and the dry basis content of silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C for 2 hours in a nitrogen atmosphere. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 1 hour in an argon atmosphere. The above materials are kept at a constant temperature of 650°C in an air atmosphere for 1 hour to obtain calcium-based CO 2 Adsorbent.
[0066] Comparative Example 2
[0067] SiC fine powder, aluminum oxide, yttrium oxide and carbon black are mixed and ground to obtain a material stream A. Based on the mass of the SiC fine powder, aluminum oxide is 5%, yttrium oxide is 2% and carbon black is 10%.
[0068] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then stream A is slowly added, and then silica sol is slowly added. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 5:1, the weight ratio of stream A to calcium nitrate is 0.1:1, and the dry basis content of silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C for 2 hours in a nitrogen atmosphere. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 3 hours in an argon atmosphere. The above materials are kept at a constant temperature of 650°C in an air atmosphere for 1 hour to obtain calcium-based CO 2 Adsorbent.
[0069] Comparative Example 3
[0070] Hexamethylenetetramine was added to deionized water containing 50% propanol, stirred rapidly, ethyl orthosilicate was slowly added, and the pH was adjusted to 8-9 with aqueous ammonia to obtain stream A. Activated carbon (specific surface area of about 700 m 2 / g), nickel nitrate and zirconium nitrate are slowly added into feed stream A. Based on the mass of tetraethyl orthosilicate, the content of hexamethylenetetramine is 15%, the content of nickel nitrate is 0.15%, the content of zirconium nitrate is 9%, and the mass ratio of activated carbon to tetraethyl orthosilicate is 1:1. Dry at 120°C, and then keep the temperature at 350°C in a hydrogen atmosphere for 10 hours to obtain feed stream B.
[0071] Calcium nitrate was slowly added to deionized water, stirred rapidly, and then stream B was slowly added, and then silica sol was slowly added. The mass ratio of the solvent to calcium nitrate was 15:1, the weight ratio of stream B to calcium nitrate was 0.35:1, and the dry content of silica sol was 0.5%. The above materials were prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 1700°C in an argon atmosphere for 7 hours. The above materials were kept at a constant temperature of 650°C in an air atmosphere for 1 hour to obtain calcium-based CO 2 Adsorbent.
[0072] Comparative Example 4
[0073] Hexamethylenetetramine was added to deionized water containing 50% propanol, and the mixture was stirred rapidly. Tetraethyl orthosilicate was slowly added, and the pH was adjusted to 8-9 with aqueous ammonia to obtain stream A. Nickel nitrate and zirconium nitrate were slowly added to stream A. Based on the mass of tetraethyl orthosilicate, the content of hexamethylenetetramine was 15%, the content of nickel nitrate was 0.15%, and the content of zirconium nitrate was 9%. The mixture was then kept at a constant temperature of 350° C. for 10 hours in a hydrogen atmosphere to obtain stream B.
[0074] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then stream B is slowly added, and then silica sol is slowly added. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 15:1, the weight ratio of stream B to calcium nitrate is 0.1:1, and the dry basis content of silica sol is 0.5%. The above materials are prepared into microspheres, dried at 120°C, and then kept at a constant temperature of 600°C for 2 hours in a nitrogen atmosphere. The above materials are sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 1 hour in an argon atmosphere. The above materials are kept at a constant temperature of 650°C in an air atmosphere for 1 hour to obtain calcium-based CO 2 Adsorbent.
[0075] Adsorbent performance evaluation:
[0076] Examples 1-4 and Comparative Examples 1-4 were used to prepare calcium-based CO 2The mass wear rate of the adsorbent was measured using a KM-5A particle wear tester with a measuring speed of 25 r / min and a test time of 10 h. The results are shown in Table 1.
[0077] Examples 1-4 and Comparative Examples 1-4 were used to prepare calcium-based CO 2 CO of adsorbent 2 The adsorption capacity was measured by thermogravimetric analyzer (TGA) under the following conditions: adsorption temperature was 650 °C, desorption temperature was 800 °C, the number of cycles was 100, and the average value was taken. 2 The adsorption capacity results are shown in Table 1.
[0078] Table 1 Mass wear rate of adsorbent and CO of adsorbent 2 Adsorption capacity
[0079] serial number Mass wear rate / % <