Thermoplastic cellular board as well as preparation method and application thereof
By using continuous fiber reinforced thermoplastic composite sheet and modified resin film in the surface structure of the thermoplastic honeycomb panel, the problem of poor edge sealing in the existing technology is solved, and the beautiful edge wrapping, sealing and mechanics of the honeycomb panel are achieved. Performance improvements.
Patent Information
- Application Number
- CN202410506373.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-25
AI Technical Summary
Existing thermoplastic honeycomb panels are prone to resin adhesion during the edge sealing process, resulting in poor appearance and are not suitable for batch processing. It is also difficult to achieve the requirements of flame retardancy, anti-aging and uniform appearance.
It adopts a surface layer structure that completely wraps the honeycomb core, including the upper layer, lower layer and side layer, each composed of continuous fiber reinforced thermoplastic composite sheet and modified resin film. Through specific matrix resin ratio and process treatment, the honeycomb is realized Effective wrapping and sealing of the core.
It achieves beautiful edge wrapping, good sealing and resistance to edge collapse of the honeycomb panel, and improves its flame retardancy, anti-aging and mechanical properties, especially the compressive and bending strength.
Smart Images

Figure CN118849531A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a thermoplastic honeycomb panel and a preparation method and application thereof. Background Art
[0002] Thermoplastic composite honeycomb panels have been widely used in rail transit, logistics, construction materials, electronics and other fields due to their light weight, high rigidity, impact resistance, moisture resistance, and recyclability. However, due to the special processing technology of the honeycomb core, it has a hollow structure and is difficult to meet the requirements of flame retardancy, anti-aging, and uniform appearance.
[0003] CN107379726A sets an edge sealing area outside the product outline, inserts a high-temperature component between the upper and lower skins of the edge in the edge sealing area, melts and removes the honeycomb and softens the upper and lower skins, and then folds the upper and lower skins toward the middle to achieve the edge sealing of the product. This edge sealing method makes the edge of the product full and firm, increases the edge strength of the product, solves the problem of edge sealing of PPHC materials, and aims to promote the application of PPHC in spare tire covers. However, this processing method removes the honeycomb with hot melt components, which is easy to adhere to the resin, resulting in poor appearance, and is not suitable for batch processing.
[0004] Patent CN113844111A discloses a honeycomb panel with edge banding and its preparation method. The upper and lower skins of the honeycomb panel are made of continuous fiber reinforced thermoplastic composite materials, the upper skin surface is provided with a coating surface and a protective film, the middle structure is a polypropylene honeycomb core, and polypropylene edge banding strips are arranged on both sides of the honeycomb core. The edge banding strips are lock-type, which can solve the problem that there is a certain gap between the two edge banding materials when the finished product is composited; a preparation method is also provided: the upper and lower surfaces are made of continuous fiber reinforced thermoplastic materials, and the upper and lower surfaces are composited with the honeycomb core through a thermal composite process to prepare a honeycomb panel; the edge banding material is circulated on both sides of the honeycomb core so that the edge of each honeycomb core is in contact with the edge banding material; the working parameters of the composite machine are set, the equipment is heated and kept warm for a fixed time, and the honeycomb panel with the edge banding material is sent to the composite machine through a conveyor belt for thermoplastic composite to obtain a honeycomb panel with edge banding. The edge banding honeycomb panel prepared by this scheme has edge banding materials only on both sides.
[0005] Therefore, how to perform edge wrapping on the honeycomb core has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a thermoplastic honeycomb panel and a preparation method and application thereof. The thermoplastic honeycomb core can effectively wrap the honeycomb core, the wrapping is beautiful, the sealing is good, it is not easy to collapse the edge, and it has excellent mechanical properties and bonding strength.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A thermoplastic honeycomb panel comprises a honeycomb core and a surface layer completely covering the outer surface of the honeycomb core, wherein the surface layer comprises an upper layer, a lower layer and a side layer;
[0009] The upper layer, the lower layer and the side layer each independently comprise a continuous fiber reinforced thermoplastic composite sheet and a modified resin film;
[0010] The continuous fiber reinforced thermoplastic composite sheet comprises continuous fibers and a matrix resin;
[0011] The base resin comprises the following components in parts by weight: 76 to 91 parts of polypropylene resin, 4.5 to 10.5 parts of toughening agent, 4.5 to 10.5 parts of compatibilizer, 0.28 to 0.82 parts of antioxidant, and 0.18 to 0.82 parts of lubricant;
[0012] The honeycomb core includes a plurality of honeycomb units arranged in an array, and the honeycomb unit includes a resin layer and an adhesive layer arranged in sequence from the inside to the outside.
[0013] Preferably, the weight ratio of the continuous fiber to the matrix resin is (4-7):(3-6).
[0014] Preferably, the upper layer extends downward to form a first bending portion, and the lower layer extends upward to form a second bending portion, and the first bending portion and the second bending portion constitute the side layer.
[0015] Preferably, the upper layer is arranged in parallel with the lower layer, and the upper layer is arranged perpendicular to the side layer.
[0016] Preferably, at least one of the following (a) to (c) is satisfied:
[0017] (a) the polypropylene resin in the matrix resin is copolymerized polypropylene, and the melt index of the copolymerized polypropylene at 230°C / 2.16kg is 60-120g / 10min;
[0018] (b) the toughening agent is at least one of a GMA grafted polyolefin resin thermoplastic elastomer and a MAH grafted polyolefin resin thermoplastic elastomer, and the toughening agent has a melt index of 1.5 to 15 g / 10 min at 190° C. / 2.16 kg;
[0019] (c) The compatibilizer in the matrix resin is MAH grafted polypropylene, the grafting rate of MAH in the MAH grafted polypropylene is 0.9-1.2%, and the melt index of the compatibilizer under the conditions of 190°C / 2.16kg is 80-120g / 10min.
[0020] The grafting rate of MAH can be determined by infrared spectroscopy: a sample of fixed thickness is tested by Fourier infrared spectrometer to obtain characteristic absorption peaks of infrared spectrum, and the grafting rate of MAH can be calculated by comparing the ratio of carbonyl and methylene absorption intensities.
[0021] Preferably, at least one of the following (1) to (3) is satisfied:
[0022] (1) The weight ratio of the resin layer to the adhesive layer is (5-10):1.
[0023] (2) The resin layer is a polyolefin resin, and the crystallinity of the polyolefin resin is 50 to 85%;
[0024] (3) The modified resin film comprises the following components in parts by weight: 75 to 90 parts of polypropylene resin, 5 to 10 parts of a compatibilizer, 5 to 10 parts of a polyolefin resin thermoplastic elastomer, and 0.1 to 0.6 parts of an anti-ultraviolet agent.
[0025] Preferably, the thickness of the continuous fiber reinforced thermoplastic composite sheet is 0.3 to 1.2 mm;
[0026] The thickness ratio of the continuous fiber reinforced thermoplastic composite sheet and the modified resin film is (30-120): (2-15).
[0027] The present invention also provides a method for preparing a thermoplastic honeycomb panel, comprising the following steps:
[0028] The upper layer, the honeycomb core and the lower layer are laid in order and compounded at 120-250° C. to obtain a honeycomb panel;
[0029] The honeycomb panel is processed with Teflon tape to make the static friction coefficient of the honeycomb panel surface ≥0.8 and the dynamic friction coefficient ≥0.17;
[0030] The honeycomb panel is cut into semi-finished honeycomb panels, the sides of the semi-finished honeycomb panel are cut, the upper layer is folded downwards and the lower layer is folded upwards in sequence, the edge sealing area is baked, and after the edge sealing area is softened, the upper and lower edge sealing areas are folded toward the middle in sequence to form side layers, and after cooling and compacting, a thermoplastic honeycomb panel is obtained.
[0031] The present invention also provides an application of a thermoplastic honeycomb panel in the fields of rail transportation, logistics transportation, building materials and construction, and electronics.
[0032] The beneficial effects of the present invention are as follows: (1) By arranging a surface layer on the outer surface of the honeycomb core, the present invention can effectively wrap the honeycomb core, which has beautiful wrapping, good sealing, and is not easy to collapse. At the same time, the materials of the upper layer, the lower layer and the side layer are consistent, which can effectively protect the honeycomb core and improve its sealing effect, so that the honeycomb panel has flame retardant, anti-aging and waterproof effects, and at the same time, greatly improves the compressive and bending strength of the honeycomb panel. (2) By using a specific matrix resin as the material of the continuous fiber reinforced thermoplastic composite sheet in the upper layer, the lower layer and the side layer, the mechanical properties and bonding strength can be effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic structural diagram of the thermoplastic honeycomb panel of the present invention.
[0034] Figure 2 Another schematic structural diagram of the thermoplastic honeycomb panel of the present invention.
[0035] Figure 3 It is a schematic diagram of cutting the side surface of the semi-finished honeycomb panel of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0037] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0038] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0039] See also Figure 1 , Figure 2 The present invention provides a thermoplastic honeycomb panel, comprising a honeycomb core 1 and a surface layer completely wrapping the outer surface of the honeycomb core 1, wherein the surface layer comprises an upper layer 2, a lower layer 3, and a side layer 4;
[0040] The upper layer, the lower layer and the side layer each independently comprise a continuous fiber reinforced thermoplastic composite sheet and a modified resin film;
[0041] The continuous fiber reinforced thermoplastic composite sheet comprises continuous fibers and a matrix resin;
[0042] The base resin comprises the following components in parts by weight: 76 to 91 parts of polypropylene resin, 4.5 to 10.5 parts of toughening agent, 4.5 to 10.5 parts of compatibilizer, 0.28 to 0.82 parts of antioxidant, and 0.18 to 0.82 parts of lubricant;
[0043] The honeycomb core includes a plurality of honeycomb units arranged in an array, and the honeycomb unit includes a resin layer and an adhesive layer arranged in sequence from the inside to the outside.
[0044] The present invention can effectively wrap the honeycomb core by arranging a surface layer on the outer surface of the honeycomb core. The wrapping is beautiful, has good sealing performance, and is not easy to collapse. At the same time, the materials of the upper layer, the lower layer and the side layer are consistent, which can effectively protect the honeycomb core and improve its sealing effect. The honeycomb panel has flame retardant, anti-aging and waterproof effects, and at the same time, the compression and bending strength of the honeycomb panel are greatly improved.
[0045] By using the above-mentioned specific matrix resin as the material of the continuous fiber reinforced thermoplastic composite sheet in the upper layer, the lower layer and the side layer, the mechanical properties and the bonding strength can be effectively improved.
[0046] In one embodiment, the weight ratio of the continuous fiber to the matrix resin is (4-7):(3-6).
[0047] In one embodiment, the upper layer extends downward to form a first bending portion 101, and the lower layer extends upward to form a second bending portion 102, and the first bending portion and the second bending portion constitute the side layer.
[0048] In one embodiment, the upper layer is arranged in parallel with the lower layer, and the upper layer is arranged perpendicular to the side layer.
[0049] In one embodiment, the base resin includes the following components in parts by weight: 80 to 90 parts of polypropylene resin, 5 to 10 parts of toughening agent, 5 to 10 parts of compatibilizer, 0.3 to 0.8 parts of antioxidant, and 0.2 to 0.8 parts of lubricant.
[0050] In one embodiment, the base resin includes the following components in parts by weight: 85 to 89.5 parts of polypropylene resin, 5 to 8 parts of toughening agent, 5 to 6 parts of compatibilizer, 0.3 to 0.5 parts of antioxidant, and 0.2 to 0.5 parts of lubricant.
[0051] In one embodiment, the weight ratio of the continuous fiber to the matrix resin is (4-7):(3-6), for example, 4:6, 5:5, 6:7, 7:3 or a range consisting of any two weight ratios thereof.
[0052] In one embodiment, at least one of the following (a) to (c) is satisfied:
[0053] (a) the polypropylene resin in the matrix resin is copolymer polypropylene, and the melt index of the copolymer polypropylene at 230°C / 2.16kg is 60 to 120 g / 10min, for example, 60 g / 10min, 70 g / 10min, 80 g / 10min, 90 g / 10min, 100 g / 10min, 110 g / 10min, 120 g / 10min or a range consisting of any two of the values;
[0054] (b) the toughening agent is at least one of a GMA grafted polyolefin resin thermoplastic elastomer and a MAH grafted polyolefin resin thermoplastic elastomer, and the melt index of the toughening agent at 190°C / 2.16kg is 1.5 to 15 g / 10min, for example, 1.5 g / 10min, 2 g / 10min, 4 g / 10min, 5 g / 10min, 6 g / 10min, 8 g / 10min, 10 g / 10min, 12 g / 10min, 15 g / 10min, or a range consisting of any two of the values;
[0055] (c) The compatibilizer in the matrix resin is MAH grafted polypropylene, the grafting rate of MAH in the MAH grafted polypropylene is 0.9-1.2%, and the melt index of the compatibilizer under the conditions of 190°C / 2.16kg is 80-120g / 10min, for example, it can be 80g / 10min, 90g / 10min, 100g / 10min, 110g / 10min, 120g / 10min or a range consisting of any two of the values.
[0056] In one embodiment, the antioxidant is at least one of a hindered phenol antioxidant, a thioether antioxidant, a polyaromatic amine antioxidant, a hindered amine antioxidant, and a phosphite antioxidant.
[0057] In one embodiment, the lubricant is at least one of pentaerythritol stearate, ethylene bisstearamide, montan wax, stearic acid, and hyperbranched polyester.
[0058] The inventors of the present invention have found that by using the above-mentioned specific copolymer polypropylene, toughening agent and compatibilizer as the material of the base resin, the bonding strength and compression strength of the honeycomb panel are effectively improved.
[0059] In one embodiment, the continuous fiber is at least one of E glass fiber unidirectional fiber yarn and E glass fiber fabric; in the continuous fiber, the weight percentage of volatile matter is not more than 0.1%, the weight percentage of film-forming agent is 0.15-0.45%, the weight percentage of compatibilizer is 0.05-0.15%, the weight percentage of coupling agent is 0.04-0.15%, and the weight ratio percentage of additives is 0.01-0.05%.
[0060] In one embodiment, the film-forming agent includes at least one of amino-modified epoxy resin and cross-linked polyurethane, the compatibilizer includes a silane coupling agent, and the additive includes at least one of polypropylene wax and polyethylene wax.
[0061] In one embodiment, the weight ratio of the resin layer to the adhesive layer is (5-10):1, for example, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two weight ratios thereof.
[0062] In one embodiment, the resin layer is a polyolefin resin, and the crystallinity of the polyolefin resin is 50-85%, for example, it can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or a range consisting of any two values therein.
[0063] In one embodiment, the polyolefin resin has a crystallinity of 60 to 80%.
[0064] In one embodiment, the polyolefin resin has a crystallinity of 60 to 70%.
[0065] In one embodiment, the polyolefin resin is at least one of polypropylene and modified polypropylene.
[0066] In one embodiment, the modified polypropylene includes the following components in parts by weight: 99.6 to 99.8 parts of polypropylene resin and 0.2 to 0.4 parts of a nucleating agent.
[0067] The present invention adopts polypropylene with high crystallinity, so as to improve the rigidity of the whole honeycomb panel and significantly improve the heat-resistant compression strength of the honeycomb panel.
[0068] In one embodiment, the adhesive layer is a polyolefin resin thermoplastic elastomer.
[0069] In one embodiment, the modified resin film comprises the following components in parts by weight: 78 to 90 parts of polypropylene resin, 5 to 10 parts of a compatibilizer, 5 to 10 parts of a polyolefin resin thermoplastic elastomer, and 0.1 to 0.6 parts of an anti-ultraviolet agent.
[0070] It should be noted that the polyolefin resin thermoplastic elastomer (POE) mentioned herein is a thermoplastic elastomer obtained by in-situ polymerization of ethylene and α-olefin, wherein the α-olefin includes at least one of α-olefins having 4 to 8 carbon atoms.
[0071] In one embodiment, the α-olefin includes at least one of 1-butene, 1-hexene, and 1-octene.
[0072] Furthermore, the polyolefin elastomer is a thermoplastic elastomer obtained by in-situ polymerization of ethylene and 1-octene.
[0073] The compatibilizer in the modified resin film is MAH grafted polypropylene, the grafting rate of MAH in the MAH grafted polypropylene is 0.9-1.2%, and the melt index of the compatibilizer under the conditions of 190°C / 2.16kg is 80-120g / 10min.
[0074] The polypropylene resin in the modified resin film has a melt index of 9 to 160 g / 10 min at 230° C. / 2.16 kg.
[0075] In one embodiment, the anti-ultraviolet agent is at least one of hydroxybenzophenones, hydroxybenzotriazoles, hydroxybenzotriazines, cyanoacrylates, and nano-scale inorganic materials (eg, titanium oxide, cerium oxide, and zinc oxide).
[0076] In one embodiment, the continuous fiber reinforced thermoplastic composite sheet has a thickness of 0.3-1.2 mm, for example, 0.3 mm, 0.4 mm, 0.6 mm, 0.8 mm, 1 mm, 1.2 mm or a range consisting of any two values therein.
[0077] In one embodiment, the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet and the modified resin film is (30-120):(2-15).
[0078] In one embodiment, the thickness of the modified resin film is 20 to 150 μm, for example, 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 150 μm or a range consisting of any two of these values.
[0079] In one embodiment, the thickness of the thermoplastic honeycomb panel is 5 to 30 mm, for example, 5 mm, 6 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm or a range consisting of any two values therein.
[0080] In one embodiment, the present invention further provides a method for preparing a thermoplastic honeycomb panel, comprising the following steps:
[0081] Providing an upper layer including a continuous fiber reinforced thermoplastic composite sheet 21 and a modified resin film 22 and a lower layer including a continuous fiber reinforced thermoplastic composite sheet 31 and a modified resin film 32, compounding them at 120-250° C. to obtain a honeycomb panel;
[0082] The honeycomb panel is processed with Teflon tape to make the static friction coefficient of the honeycomb panel surface ≥0.8 and the dynamic friction coefficient ≥0.17;
[0083] Cut the honeycomb panels into semi-finished honeycomb panels, such as Figure 3 As shown, the side of the semi-finished honeycomb panel is cut, the upper layer is folded downward and the lower layer is folded upward in sequence, the edge sealing area is baked, and after the edge sealing area is softened, the upper and lower edge sealing areas are folded toward the middle in sequence to form side layers, which are then cooled and compacted to obtain a thermoplastic honeycomb panel.
[0084] The cutting width range is: final product width + 1 / 2 product thickness ~ final product width + product thickness; the cutting length range is: final product length + 1 / 2 product thickness ~ final product length + product thickness.
[0085] Cut the honeycomb core from the side, the cutting depth is 1 / 2 product thickness ~ product thickness, the reserved thickness of the honeycomb core on the upper and lower surfaces is 1 / 10 honeycomb core thickness ~ 1 / 2 honeycomb core thickness. According to the different thickness of honeycomb core, the thickness of the milling cutter can be changed to obtain grooves of different depths and cutting thicknesses.
[0086] In one embodiment, the present invention further provides an application of the thermoplastic honeycomb panel in the fields of rail transportation, logistics and transportation, building materials and construction, and electronics.
[0087] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0088] The raw materials used in the embodiments and comparative examples are described as follows:
[0089] Copolymer PP-1: Copolymer polypropylene, the melt index at 230℃ / 2.16kg is 80g / 10min, manufacturer: Yanshan Petrochemical, brand: K7780.
[0090] Copolymer PP-2: Copolymer polypropylene, the melt index at 230℃ / 2.16kg is 60g / 10min, manufacturer: Yanshan Petrochemical, brand: K7760H.
[0091] Copolymer PP-3: Copolymer polypropylene, the melt index at 230℃ / 2.16kg is 120g / 10min, manufacturer: South Korea SK, brand: BX3920 / BX3950 mixed in a ratio of 7:3.
[0092] Toughening agent-1: GMA grafted POE, the melt index at 190℃ / 2.16kg is 1.5g / 10min, manufacturer: Guangdong Chuanheng, brand: CH-904.
[0093] Toughening agent-2: GMA grafted POE, the melt index at 190℃ / 2.16kg is 15g / 10min, manufacturer: Mingyuan, brand: W5E.
[0094] Toughening agent-3: GMA grafted POE, the melt index at 190℃ / 2.16kg is 5g / 10min, manufacturer: Jiayirong, brand: SOG-02.
[0095] Toughening agent-4: MAH grafted POE, the melt index at 190℃ / 2.16kg is 3.3g / 10min, manufacturer: Dow, USA, brand: GR208.
[0096] Compatibilizer-1: MAH grafted polypropylene, the grafting rate of MAH is 1.0%, the melt index of the compatibilizer under the conditions of 190°C / 2.16kg is 100g / 10min, manufacturer: Ployram, brand: Bondyram1001.
[0097] Antioxidant: Manufacturer: Sanfeng Chemical, brand: Sonox225G.
[0098] Lubricant: Manufacturer: Wuhan Hyperbranched Chemical, Brand: HBP-158.
[0099] Continuous fiber: Manufacturer: China Jushi Co., Ltd., Brand: EDR16-1200-362A(U).
[0100] PP-1: modified homopolypropylene (obtained by extrusion granulation of homopolypropylene resin and 2% sodium benzoate nucleating agent): crystallinity 60%, homopolypropylene resin manufacturer: Japan Prime, brand PP / J-700GP.
[0101] PP-2: Homopolymer polypropylene resin: crystallinity 70%, manufacturer: Hanhua, brand HJ730.
[0102] PP-3: Homopolymer polypropylene resin: crystallinity 50%, manufacturer: Japan Prime, brand PP / J-700GP.
[0103] PP-4: modified homopolypropylene (obtained by extrusion granulation of homopolypropylene resin and 1% dimethylbenzylidene sorbitol): crystallinity 85%, homopolypropylene resin manufacturer: Hanhua, brand HJ730.
[0104] PP-5: Copolymer polypropylene resin: The melt index at 230℃ / 2.16kg is 9g / 10min. Manufacturer: Sinopec Qilu Petrochemical Company, brand: SP179.
[0105] PP-6: Copolymer polypropylene resin: The melt index at 230℃ / 2.16kg is 160g / 10min, manufacturer: South Korea SK, brand: BX3950.
[0106] Nucleating agent: Manufacturer: Milliken, brand: MILLAD3988.
[0107] POE: Manufacturer: Nantong Ruicheng, Brand: RC9030.
[0108] Anti-UV agent: Manufacturer: Baoxu Chemical, Brand: Light Stabilizer-UV-3808PP5.
[0109] Examples 1 to 8, Comparative Examples 1 to 4
[0110] The thermoplastic honeycomb panels of Examples 1 to 8 and Comparative Examples 1 to 4 include a honeycomb core and a surface layer completely wrapping the outer surface of the honeycomb core, wherein the surface layer includes an upper layer, a lower layer, and a side layer.
[0111] The upper layer, the lower layer and the side layers each independently comprise a continuous fiber reinforced thermoplastic composite sheet and a modified resin film.
[0112] The upper layer extends downward to form a first bending portion, and the lower layer extends upward to form a second bending portion. The first bending portion and the second bending portion constitute the side layer.
[0113] The upper layer is arranged in parallel with the lower layer, and the upper layer is arranged perpendicular to the side layer.
[0114] The continuous fiber reinforced thermoplastic composite sheet comprises continuous fibers and a matrix resin (the proportion of the matrix resin is shown in Table 1); the weight ratio of the continuous fibers to the matrix resin is 6:4;
[0115] The honeycomb core includes a plurality of honeycomb units arranged in an array, and the honeycomb unit includes a resin layer and an adhesive layer sequentially arranged from the inside to the outside, and the weight ratio of the resin layer to the adhesive layer is 8:1.
[0116] The resin layer includes the following components in parts by weight: 99.7 parts of PP-1 and 0.3 parts of a nucleating agent.
[0117] The adhesive layer is POE.
[0118] The modified resin film includes the following components in parts by weight: 85.5 parts of PP-5, 8 parts of compatibilizer-1, 6 parts of POE, and 0.5 parts of anti-ultraviolet agent.
[0119] The thickness of the continuous fiber reinforced thermoplastic composite sheet is 0.3 mm; the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet to the modified resin film is 100:10, and the thickness of the thermoplastic honeycomb panel is 10 mm.
[0120] The method for preparing the thermoplastic honeycomb panel comprises the following steps:
[0121] The upper layer, the honeycomb core and the lower layer are laid in order and compounded at 220° C. to obtain a honeycomb panel;
[0122] The honeycomb panel is processed with Teflon tape, so that the static friction coefficient of the honeycomb panel surface is 0.88 and the dynamic friction coefficient is 0.17;
[0123] Cut the honeycomb panel into semi-finished honeycomb panel square panels, such as Figure 3 As shown, the sides of the semi-finished honeycomb panel are cut, and the depth of the milling cutter is 1 / 2 thickness of the honeycomb panel to the product thickness. The upper layer is folded downwards and the lower layer is folded upwards in turn, and the edge sealing area is baked. After the edge sealing area is softened, the upper and lower edge sealing areas are folded toward the middle in turn to form side layers, which are cooled and compacted to obtain the following Figure 1 Thermoplastic honeycomb panel shown.
[0124] Table 1
[0125]
[0126] Embodiments 9 to 11
[0127] The difference between Examples 9 to 11 and Example 1 is that the polypropylene of the resin layer is different, and the other parts are the same.
[0128] The polypropylene of the resin layer of Example 9 is PP-2.
[0129] The polypropylene of the resin layer in Example 10 is PP-3.
[0130] The polypropylene of the resin layer in Example 11 is PP-4.
[0131] Embodiments 12 to 15
[0132] The difference between Examples 12 to 15 and Example 1 is that the thicknesses of the continuous fiber reinforced thermoplastic composite sheet and the modified resin film are different, and the other aspects are the same.
[0133] The thickness of the continuous fiber reinforced thermoplastic composite sheet in Example 12 is 0.9 mm, and the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet to the modified resin film is 30:2.
[0134] The thickness of the continuous fiber reinforced thermoplastic composite sheet described in Example 13 is 1.2 mm, and the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet to the modified resin film is 120:15.
[0135] The thickness of the continuous fiber reinforced thermoplastic composite sheet described in Example 14 is 1.5 mm, and the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet to the modified resin film is 120:80.
[0136] The thickness of the continuous fiber reinforced thermoplastic composite sheet described in Example 15 is 0.6 mm, and the thickness ratio of the continuous fiber reinforced thermoplastic composite sheet to the modified resin film is 30:1.
[0137] Embodiments 16 to 18
[0138] The difference between Examples 16 to 18 and Example 1 is that the thickness of the thermoplastic honeycomb panels is different, and the other aspects are the same.
[0139] The thickness of the thermoplastic honeycomb panel of Example 16 is 5 mm.
[0140] The thickness of the thermoplastic honeycomb panel of Example 17 is 15 mm.
[0141] The thickness of the thermoplastic honeycomb panel in Example 18 is 20 mm.
[0142] Embodiment 19
[0143] The difference between Example 19 and Example 1 is that the polypropylene of the modified resin film is different.
[0144] The polypropylene of the modified resin film of Example 19 is PP-6.
[0145] Comparative Example 5
[0146] The difference between Comparative Example 5 and Example 1 is that Comparative Example 5 does not contain a side layer (ie, Comparative Example 5 is not hemmed), and the other aspects are the same.
[0147] Comparative Example 6
[0148] The difference between Comparative Example 6 and Example 1 is that the side layer of Comparative Example 6 is a rubber strip (ie, Comparative Example 6 is wrapped with a rubber strip), and the rest is the same.
[0149] Test Case
[0150] Compression test: refer to GB / T 1453-2005 Test method for flat compression performance of sandwich structure or core, the speed is 0.5mm / min.
[0151] Bending test: refer to GB / T 1456-2005 Sandwich structure bending performance test method, the speed is 5mm / min.
[0152] Peel strength: Refer to GB / T 1457-2005 "Sandwich structure roller peel strength test method" for testing.
[0153] Table 2
[0154]
[0155]
[0156] It can be seen from Table 2 that the thermoplastic honeycomb panel of the present invention has excellent bending strength, compression strength and peeling strength.
[0157] The thermoplastic honeycomb panel prepared by the present invention has a compression strength of ≥1.45MPa at 23°C, a compression strength of ≥0.32MPa at 90°C, a peel strength of ≥132 (N·mm) / mm, an edge compression strength of ≥1.76MPa, an edge bending strength of ≥14.6MPa, and a bending deflection of 5mm without abnormality.
[0158] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A thermoplastic honeycomb panel, characterized in that: It includes a honeycomb core and a surface layer that completely wraps the outer surface of the honeycomb core, wherein the surface layer includes an upper layer, a lower layer, and a side layer; The upper layer, the lower layer and the side layer each independently comprise a continuous fiber reinforced thermoplastic composite sheet and a modified resin film; The continuous fiber reinforced thermoplastic composite sheet comprises continuous fibers and a matrix resin; The base resin comprises the following components in parts by weight: 76 to 91 parts of polypropylene resin, 4.5 to 10.5 parts of toughening agent, 4.5 to 10.5 parts of compatibilizer, 0.28 to 0.82 parts of antioxidant, and 0.18 to 0.82 parts of lubricant; The honeycomb core includes a plurality of honeycomb units arranged in an array, and the honeycomb unit includes a resin layer and an adhesive layer arranged in sequence from the inside to the outside.
2. The thermoplastic honeycomb panel according to claim 1, characterized in that: The weight ratio of the continuous fiber to the matrix resin is (4-7):(3-6).
3. The thermoplastic honeycomb panel according to claim 1, characterized in that: The upper layer extends downward to form a first bending portion, and the lower layer extends upward to form a second bending portion. The first bending portion and the second bending portion constitute the side layer.
4. The thermoplastic honeycomb panel according to claim 1, characterized in that: The upper layer is arranged in parallel with the lower layer, and the upper layer is arranged perpendicular to the side layer.
5. The thermoplastic honeycomb panel according to claim 1, characterized in that: Satisfy at least one of the following (a) to (c): (a) the polypropylene resin in the matrix resin is copolymerized polypropylene, and the melt index of the copolymerized polypropylene at 230°C / 2.16kg is 60-120g / 10min; (b) the toughening agent is at least one of a GMA grafted polyolefin resin thermoplastic elastomer and a MAH grafted polyolefin resin thermoplastic elastomer, and the toughening agent has a melt index of 1.5 to 15 g / 10 min at 190° C. / 2.16 kg; (c) The compatibilizer in the matrix resin is MAH grafted polypropylene, the grafting rate of MAH in the MAH grafted polypropylene is 0.9-1.2%, and the melt index of the compatibilizer under the conditions of 190°C / 2.16kg is 80-120g / 10min.
6. The thermoplastic honeycomb panel according to claim 1, characterized in that: Satisfy at least one of the following (1) to (3): (1) The weight ratio of the resin layer to the adhesive layer is (5-10):
1. (2) The resin layer is a polyolefin resin, and the crystallinity of the polyolefin resin is 50 to 85%; (3) The modified resin film comprises the following components in parts by weight: 75 to 90 parts of polypropylene resin, 5 to 10 parts of a compatibilizer, 5 to 10 parts of a polyolefin resin thermoplastic elastomer, and 0.1 to 0.6 parts of an anti-ultraviolet agent.
7. The thermoplastic honeycomb panel according to claim 1, characterized in that: The continuous fiber reinforced thermoplastic composite material sheet has a thickness of 0.3 to 1.2 mm; The thickness ratio of the continuous fiber reinforced thermoplastic composite sheet and the modified resin film is (30-120): (2-15).
8. The thermoplastic honeycomb panel according to claim 1, characterized in that: The thickness of the thermoplastic honeycomb panel is 5 to 30 mm.
9. The method for preparing a thermoplastic honeycomb panel according to any one of claims 1 to 8, characterized in that: The following steps are involved: The upper layer, the honeycomb core and the lower layer are laid in order and compounded at 120-250° C. to obtain a honeycomb panel; The honeycomb panel is processed with Teflon tape to make the static friction coefficient of the honeycomb panel surface ≥0.8 and the dynamic friction coefficient ≥0.17; The honeycomb panel is cut into semi-finished honeycomb panels, the sides of the semi-finished honeycomb panel are cut, the upper layer is folded downwards and the lower layer is folded upwards in sequence, the edge sealing area is baked, and after the edge sealing area is softened, the upper and lower edge sealing areas are folded toward the middle in sequence to form side layers, and after cooling and compacting, a thermoplastic honeycomb panel is obtained.
10. Application of the thermoplastic honeycomb panel according to any one of claims 1 to 8 in the fields of rail transportation, logistics and transportation, building materials and construction, and electronics.
Citation Information
Patent Citations
Method for sealing edge of plastic cellular sandwich board and apparatus thereof
CN107379726A
Post bending and edge covering structure of metal composite plate
CN110000252A
Honeycomb core sandwich composite board and preparation method and equipment thereof
CN111098559A
High-bonding-strength hot melt adhesive for polypropylene plastic cellular board and preparation method of high-bonding-strength hot melt adhesive
CN112852346A
Thermoplastic cellular board as well as preparation method and application thereof
CN116749603A