Vanadium sodium fluorophosphate composite material as well as preparation method and application thereof

The sodium vanadium fluorophosphate composite material is prepared by a two-step microwave sintering method, which solves the problems of poor rate performance and long-term stability, forms a loose porous structure, improves the electrochemical performance and cycle stability, and realizes efficient battery applications. .

CN118851137APending Publication Date: 2024-10-29ZIGONG DONGXIN CARBON CO LTD +1

Patent Information

Application Number
CN202410849131.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The poor rate performance and long-term stability of sodium fluorovanadium phosphate composites lead to structural collapse and low electronic conductivity under high current densities, limiting their industrial application.

Method used

A two-step microwave sintering method is used to prepare sodium vanadium fluorophosphate composite materials. Through vacuum freeze-drying and microwave calcination, a uniformly distributed loose porous material is formed, which increases the electrolyte contact area, reduces the degree of polarization, and improves the cycle performance of the material.

Benefits of technology

The capacity retention and rate performance of the sodium fluorovanadium phosphate composite material is improved. The assembled button battery has a retention rate of 93.2% after 100 cycles at 1C, and shows high electrochemical stability under different current densities. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851137A_ABST
    Figure CN118851137A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium vanadium fluorophosphate composite material as well as a preparation method and application thereof, and belongs to the technical field of material preparation. The sodium vanadium fluorophosphate precursor is subjected to vacuum freeze drying and combined with microwave sintering to prepare the sodium vanadium fluorophosphate positive electrode material, the shape of the sodium vanadium fluorophosphate positive electrode material is changed into a uniformly distributed loose porous shape from an irregular sheet shape, the surface is wrapped by an amorphous carbon layer, the preparation method is simple and convenient, and the yield is relatively high. Microwave sintering can realize overall heating of the material, vanadium sodium fluorophosphate is prepared by regulating and controlling the temperature, so that the scale-shaped material is obtained, and along with a surface porous structure, the contact area of an electrolyte is increased, and more sufficient infiltration is beneficial to reduction of the polarization degree during oxidation-reduction reaction; the capacity retention rate and the rate capability of the sodium vanadium fluorophosphate composite material are improved, and the retention rate of an assembled button cell can reach 93.2% after 100 cycles under the condition of 1C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a sodium vanadium fluorophosphate composite material and a preparation method and application thereof. Background Art

[0002] The positive electrode materials of sodium ion batteries and lithium ion batteries are important components of energy storage systems. Therefore, the positive electrode materials must have the advantages of high capacity, high stability, long cycle life and good safety performance. Sodium vanadium fluorophosphate is a polyanion material, a typical NASICON material. The [PO4] tetrahedral unit and the strong inductive effect of F provide it with a stable three-dimensional skeleton structure and a stable diffusion channel for sodium ions. At the same time, the high voltage platform enables the material to have high energy density and excellent rate performance. However, the insertion / deinsertion of sodium ions causes structural deformation, which reduces the electrochemical stability of the material and even collapses the structure at high current density. In addition, the presence of [PO4] brings the problem of low intrinsic electronic conductivity of sodium vanadium fluorophosphate, which seriously limits the rate performance and long cycle stability, and hinders the further industrial application of sodium vanadium fluorophosphate composite materials. At present, the electrochemical properties of sodium vanadium fluorophosphate composites are improved by doping, carbon coating, and crystal structure regulation. These modification methods are more often prepared by combining the sol-gel method with high-temperature sintering, but there are problems such as high energy consumption that need further exploration. Therefore, it is urgent to find a more efficient and energy-saving process. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a sodium vanadium fluorophosphate composite material and a preparation method and application thereof, so as to solve the technical problem that the sodium vanadium fluorophosphate composite material has poor rate performance and long-term stability.

[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a sodium vanadium fluorophosphate composite material, comprising the following steps:

[0005] S1, dissolving a vanadium source, a phosphorus source, a sodium source, a fluorine source and a reducing agent in water at a mass ratio / molar ratio of 1-3:1-3:2-4:2-4:2-4, and then reacting at 60-80°C for 30-50 minutes. After the reaction is completed, freeze-drying the reaction solution to obtain a precursor;

[0006] S2. The precursor is calcined by a two-step microwave sintering method. The precursor is placed in an inert atmosphere and calcined at 300-400° C. for 0.5-1.5 h, and then the temperature is raised to 650-800° C. for a second calcination for 1.5-2.5 h to obtain a sodium vanadium fluorophosphate composite material.

[0007] On the basis of the above technical solution, the present invention can also be improved as follows:

[0008] Furthermore, the vanadium source is ammonium metavanadate, sodium metavanadate or vanadium pentoxide; the phosphorus source is ammonium dihydrogen phosphate, sodium dihydrogen phosphate, sodium hypophosphite or phosphoric acid; the sodium source is sodium metavanadate, sodium dihydrogen phosphate, sodium hypophosphite or sodium fluoride; the fluorine source is sodium fluoride or ammonium bifluoride; and the reducing agent is citric acid.

[0009] Furthermore, the mass ratio / molar ratio of the vanadium source, the phosphorus source, the sodium source, the fluorine source and the reducing agent is 2:2:3:3:3.

[0010] Furthermore, the reaction temperature was 70° C. and the reaction time was 40 min.

[0011] Furthermore, before freeze drying, the reaction solution is placed at -40 to 0° C. and frozen for 4 to 6 hours.

[0012] Furthermore, the vacuum degree of freeze drying is 0 to 10 Pa, the temperature is -60 to -40°C, and the time is 20 to 30 hours.

[0013] Furthermore, the heating rates during the primary calcination and the secondary calcination are both 3-7°C / min.

[0014] Furthermore, the temperature of the first calcination is 350° C., and the time of the first calcination is 1 h; the temperature of the second calcination is 700° C., and the time of the second calcination is 2 h.

[0015] The invention also discloses a sodium vanadium fluorophosphate composite material prepared by the preparation method.

[0016] The invention also discloses the application of the sodium vanadium fluorophosphate composite material in the preparation of anode materials for batteries.

[0017] The beneficial effects of the present invention are as follows: the present invention prepares the sodium vanadium fluorophosphate positive electrode material by vacuum freeze drying of the sodium vanadium fluorophosphate precursor and microwave sintering, and the morphology thereof is transformed from irregular flakes to uniformly distributed loose porous type, and the surface is wrapped with an amorphous carbon layer, and the preparation method is simple and the yield is high. Microwave sintering can realize the overall heating of the material, and the sodium vanadium fluorophosphate is prepared by regulating the temperature, thereby obtaining a flaky material, and the porous structure on the surface increases the contact area of ​​the electrolyte, and more sufficient infiltration is conducive to reducing the polarization degree during the redox reaction, and improving the capacity retention rate and rate performance of the sodium vanadium fluorophosphate composite material. The assembled button battery can achieve a retention rate of 93.2% after 100 cycles under 1C conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The X-ray diffraction pattern of the sodium vanadium fluorophosphate composite material prepared in Example 3;

[0019] Figure 2 This is a scanning electron microscope photograph of the sodium vanadium fluorophosphate composite material prepared in Example 3;

[0020] Figure 3 The charge and discharge curves of the sodium vanadium fluorophosphate composite materials (samples #1 to #4) prepared in Examples 3 to 6 after 100 cycles at a current density of 1C;

[0021] Figure 4 The charge-discharge curve of the sodium vanadium fluorophosphate composite material (sample #5) prepared in the comparative example after 100 cycles at a current density of 1C;

[0022] Figure 5 The charge and discharge curves of the sodium vanadium fluorophosphate composite materials (samples #1 to #4) prepared in Examples 3 to 6 after 10 cycles at a current density of 0.2 to 20C;

[0023] Figure 6 The charge and discharge curves of the sodium vanadium fluorophosphate composite material (sample #5) prepared in the comparative example after 10 cycles at a current density of 0.2 to 20C. DETAILED DESCRIPTION

[0024] The specific embodiments of the present invention are described below to facilitate the understanding of the present invention by those skilled in the art. If the specific conditions are not specified in the examples, the methods are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. However, it should be clear that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

[0025] Example 1

[0026] A method for preparing a sodium vanadium fluorophosphate composite material comprises the following steps:

[0027] S1. Dissolve 1 g of sodium metavanadate, 3 g of sodium dihydrogen phosphate, 4 g of ammonium bifluoride and 2 g of citric acid in 50 mL of water, and then react at 60°C for 50 min. After the reaction, freeze the reaction solution at -40°C for 4 h, and then freeze-dry the frozen solid at 0 Pa and -60°C for 20 h to obtain a precursor.

[0028] S2. Place the precursor in an argon atmosphere, first increase the temperature from room temperature to 300°C at a heating rate of 3°C / min, and calcine at this temperature for 1.5 hours, then continue to increase the temperature to 800°C at a heating rate of 7°C / min, and calcine for a second time for 1.5 hours to obtain a sodium vanadium fluorophosphate composite material.

[0029] Example 2

[0030] A method for preparing a sodium vanadium fluorophosphate composite material comprises the following steps:

[0031] S1. Dissolve 3g of vanadium pentoxide, 1g of phosphoric acid, 4g of sodium dihydrogen phosphate, 4g of ammonium bifluoride and 2g of citric acid in 50mL of water, and then react at 80°C for 30min. After the reaction, freeze the reaction solution at 0°C for 6h, and then freeze-dry the frozen solid at 10Pa and -40°C for 30h to obtain a precursor;

[0032] S2. Place the precursor in a nitrogen atmosphere, first increase the temperature from room temperature to 400°C at a heating rate of 7°C / min, and calcine at this temperature for 0.5h, then continue to increase the temperature to 700°C at a heating rate of 3°C / min, and calcine for a second time for 2.5h to obtain a sodium vanadium fluorophosphate composite material.

[0033] Example 3

[0034] A method for preparing a sodium vanadium fluorophosphate composite material comprises the following steps:

[0035] S1. Dissolve 2 g of ammonium metavanadate, 2 g of ammonium dihydrogen phosphate, 1 g of sodium metavanadate, 3 g of sodium fluoride and 3 g of citric acid in 50 mL of water, and then react at 70 ° C for 40 min. After the reaction, freeze the reaction solution at -2 ° C for 5 h, and then freeze-dry the frozen solid at 5 Pa and -50 ° C for 25 h to obtain a precursor;

[0036] S2. Place the precursor in argon gas, first increase the temperature from room temperature to 350°C at a heating rate of 5°C / min, and calcine at this temperature for 1 hour, then continue to increase the temperature to 650°C at a heating rate of 5°C / min, and calcine for a second time for 2 hours to obtain a sodium vanadium fluorophosphate composite material (sample #1).

[0037] Figure 1 is the X-ray diffraction pattern of the sodium vanadium fluorophosphate composite material (sample #1), Figure 2 This is a scanning electron microscope photo of the sodium vanadium fluorophosphate composite material (sample #1). It can be seen from the figure that the sodium vanadium fluorophosphate composite material is in the form of continuously distributed scales, and some materials are accompanied by a porous structure, which is conducive to the penetration of the electrolyte.

[0038] Example 4

[0039] The difference between this embodiment and embodiment 3 is that the temperature of the secondary calcination is adjusted to 700° C., and the other implementation conditions are the same as those of embodiment 3, to obtain a sodium vanadium fluorophosphate composite material (sample #2).

[0040] Example 5

[0041] The difference between this embodiment and embodiment 3 is that the temperature of the secondary calcination is adjusted to 750° C., and the other implementation conditions are the same as those of embodiment 3, thereby obtaining a sodium vanadium fluorophosphate composite material (sample #3).

[0042] Example 6

[0043] The difference between this embodiment and embodiment 3 is that the temperature of the secondary calcination is adjusted to 800° C., and the other implementation conditions are the same as those of embodiment 3, thereby obtaining a sodium vanadium fluorophosphate composite material (sample #4).

[0044] Comparative Example

[0045] The difference between this comparative example and Example 4 is that: 2g of ammonium metavanadate, 2g of ammonium dihydrogen phosphate, 1g of sodium metavanadate, 3g of sodium fluoride and 3g of citric acid are dissolved in 50mL of water, then placed at 80°C for reaction for 40min, slowly stirred until gel state, and after the reaction is completed, the reaction solution is dried at 60°C for 12h to obtain a precursor;

[0046] The remaining implementation conditions were the same as those in Example 3 to obtain a sodium vanadium fluorophosphate composite material (sample #5).

[0047] Experimental example

[0048] The samples (#1-#4), acetylene black and binder were mixed in a mass ratio of 7:1:1, and the solvent N-methylpyrrolidone was added and continuously ground to obtain a mixed viscous slurry. The mixed slurry was evenly coated on the cut conductive current collector (aluminum foil), placed in a vacuum drying oven, dried at 80°C for 12h, and then cut into small discs of Φ12mm as the positive electrode; the positive electrode material and the negative electrode material (sodium metal sheet), glass fiber paper (Whatman, GF / A) separator and electrolyte were assembled into a battery in an argon-filled glove box and the electrochemical performance was tested. The voltage range was 2-4.5V, the cycle condition was 1C, and the rate conditions were 0.2C, 0.5C, 1C, 2C, 5C, 10C and 20C. The test results are shown in Table 1.

[0049] Table 1 First discharge specific capacity of positive electrode materials prepared by samples #1 to #5

[0050] Example 3 Example 4 Example 5 Example 6 Comparative Example Sample No. #1 #2 #3 #4 #5 Discharge specific capacity (%) 85.5 92.1 78.7 82.9 83.91 Coulomb efficiency (%) 89.4 86.59 89.54 70.83 68.83

[0051] The charge-discharge cycle stability of samples #1 to #5 was tested at a voltage of 2 to 4.5 V and a current density of 1 C. After 100 cycles, the results are as follows: Figure 3 and Figure 4As shown, the capacity retention rate of sample #1 is 86.9%, the capacity retention rate of sample #2 is 93.2%, the capacity retention rate of sample #3 is 92.4%, the capacity retention rate of sample #4 is 85.8%, and the capacity retention rate of sample #5 is 84.8%. The electrochemical performance of samples #1 to #4 is improved compared with that of sample #5.

[0052] The test voltage was set to 2-4.5V, and the current density was set to 0.2C, 0.5C, 1C, 2C, 5C, 10C, and 20C. After 10 cycles, the charge and discharge curves of samples #1 to #5 were as follows: Figure 5 and Figure 6 As shown in the figure, it can be seen that sample #2 has higher electrochemical stability at different current densities, and sample #5 has relatively low capacity at high current density and poor capacity retention.

Claims

1. A method for preparing a sodium vanadium fluorophosphate composite material, characterized in that: The following steps are involved: S1, dissolving a vanadium source, a phosphorus source, a sodium source, a fluorine source and a reducing agent in water at a molar ratio of 1-3:1-3:2-4:2-4:2-4, and then reacting at 60-80° C. for 30-50 min. After the reaction is completed, freeze-drying the reaction solution to obtain a precursor; S2. The precursor is placed in an inert atmosphere, first calcined at 300-400° C. for 0.5-1.5 h, and then heated to 650-800° C. for a second calcination for 1.5-2.5 h to obtain a sodium vanadium fluorophosphate composite material.

2. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: The vanadium source is ammonium metavanadate, sodium metavanadate or vanadium pentoxide; the phosphorus source is ammonium dihydrogen phosphate, sodium dihydrogen phosphate, sodium hypophosphite or phosphoric acid; the sodium source is sodium metavanadate, sodium dihydrogen phosphate, sodium hypophosphite or sodium fluoride; the fluorine source is sodium fluoride or ammonium bifluoride; and the reducing agent is citric acid.

3. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: The mass ratio / molar ratio of the vanadium source, phosphorus source, sodium source, fluorine source and reducing agent is 2:2:3:3:

3.

4. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: The reaction temperature is 70° C. and the reaction time is 40 min.

5. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: Before freeze drying, the reaction solution is placed at -40 to 0°C and frozen for 4 to 6 hours.

6. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1 or 5, characterized in that: The vacuum degree of the freeze drying is 0 to 10 Pa, the temperature is -60 to -40°C, and the time is 20 to 30 hours.

7. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: The heating rates during the primary calcination and the secondary calcination are both 3-7°C / min.

8. The method for preparing the sodium vanadium fluorophosphate composite material according to claim 1, characterized in that: The temperature of the first calcination is 350° C., and the time of the first calcination is 1 hour; the temperature of the second calcination is 700° C., and the time of the second calcination is 2 hours.

9. A sodium vanadium fluorophosphate composite material, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.

10. Use of the sodium vanadium fluorophosphate composite material according to claim 9 in preparing a positive electrode material for a battery.

Citation Information

Patent Citations

  • Process for the preparation of crystalline lithium-, iron- and phosphate-comprising materials

    CA2721204A1

  • Ball-shaped lithium-ion battery anode material doped with rare earth and method for making same

    CN101013751A

  • Preparation method of positive pole material of lithium ion battery

    CN102790203A

  • Preparation method of high-power and long-service life lithium vanadium phosphate sodium / carbon positive electrode material

    CN106684384A

  • Doping modified sodium vanadium fluorophosphates positive electrode material and preparation method thereof

    CN108899505A

Cited By

  • Seamless fitting processing technology for sectioned graphite sealing ring

    CN119572598A

  • Preparation method and application of capsule-hole-rich nano spherical manganese-doped sodium vanadium fluorophosphate positive electrode material

    CN121044563A

  • Preparation method and application of a rich-pore nanospherical manganese-doped sodium vanadium fluorophosphate positive electrode material