Lightweight polyimide-based carbon foam with excellent mechanical strength and high-temperature heat-insulating property as well as preparation method and application of lightweight polyimide-based carbon foam
Polyimide-based carbon foam is prepared by copolymerizing aromatic dianhydride and aromatic diamine, which solves the problem of insufficient mechanical strength and thermal insulation performance of existing high-temperature insulation materials, and prepares lightweight materials suitable for high-temperature environments for aerospace applications. and thermal protection of high-temperature industrial equipment.
Patent Information
- Application Number
- CN202410887592.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
Existing high-temperature insulation materials have deficiencies in mechanical strength and high-temperature insulation performance. It is difficult to effectively block heat and withstand mechanical impact in harsh aerodynamic environments, and their heavy weight affects the maneuverability of the aircraft.
Polyimide precursors are prepared by copolymerizing aromatic dianhydrides and aromatic diamines, and lightweight polyimide bases with excellent mechanical strength and high-temperature thermal insulation properties are prepared through microsphere foaming, thermal imidization and high-temperature carbonization. Carbon foam.
The prepared polyimide-based carbon foam has low density, high compressive strength and low thermal conductivity. It is suitable for high-temperature environments and is suitable for thermal protection of aerospace, rocket propulsion systems and high-temperature industrial equipment. It has broad application prospects.
Smart Images

Figure CN118851148A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of materials, and in particular relates to a lightweight polyimide-based carbon foam having excellent mechanical strength and high-temperature heat insulation performance, and a preparation method and use thereof. Background Art
[0002] With the development of modern space technology, the aerodynamic thermal environment and engine-related environment faced by space exploration, atmospheric entry, and space-to-space shuttles are becoming increasingly harsh. For example, when a hypersonic vehicle is flying at high Mach for a long time in near-space, the aerodynamic heating of the fuselage surface is extremely severe; and when the spacecraft returns to the atmosphere, it will also be affected by extremely high temperatures. In order to avoid the damage of the fuselage to the harsh thermal environment, higher requirements are placed on high-temperature thermal insulation materials. High-temperature thermal insulation materials not only require excellent high-temperature thermal insulation properties, but also must have sufficient mechanical strength to block the heat on the fuselage surface from spreading to the inside of the fuselage while withstanding harsh thermal environments such as ultra-high temperatures, rapid thermal shocks, and strong vibrations. In addition, the anti-thermal insulation materials used in aircraft should also reduce their own weight as much as possible to ensure the lightweight thermal protection system and the maneuverability of the aircraft. Therefore, it is of great significance to develop lightweight materials with high mechanical strength and excellent high-temperature thermal insulation properties.
[0003] Carbon foam is a three-dimensional porous material with the characteristics of light weight, good high temperature stability and low thermal conductivity. It has broad applications in high temperature insulation and other fields. At present, the sources of carbon foam precursors are relatively wide, mainly including carbon nanomaterials, biomass and organic polymers. Carbon nanomaterials form carbon foam materials by the accumulation of nanoparticles. Although this carbon foam material has low thermal conductivity, the interaction between nanoparticles is weak and its mechanical strength is relatively low. Carbon foam materials can be obtained after heating and carbonizing biomass, but its structure and performance mainly depend on the structure of biomass. Therefore, in practical applications, biomass-based carbon foam is difficult to design specifically according to specific working conditions. Organic polymers are considered to be the best choice for carbon foam precursors because of their controllable micromorphology and chemical composition, and they show advantages such as light weight, strong structural and performance designability. Organic polymers such as melamine, phenolic resin, and polyimide have been widely studied. For example, Su Kim et al. invented a phenolic carbon foam reinforced with MWCNTs. Although the prepared carbon foam has a low thermal conductivity (~0.09 W·m -1 K -1), but the mechanical strength is relatively low, which is ~0.14MPa (Seung A Song, Youngmin Lee, Yeon Su Kim, Seong Su Kim, Mechanical and thermal properties of carbon foam derived from phenolic foam reinforced with composite particles, Composite Structures, 173 (2017) (1-8)). The polyimide segment contains a large number of benzene rings and imide ring structures, which give it excellent carbon-forming properties and is often considered as a carbon foam precursor. Ni et al. invented a polyimide-based carbon foam by microwave-assisted foaming method. The carbon foam has a low density (22.9kg·m -3 ), high temperature resistance, and excellent thermal insulation performance, the mechanical properties reach 0.10MPa (L.Ni, Z.Kang, Y.Luo, L.Yan, J.Lu, G.Wang, S.Qiu, M.Liang, S.Zhou, H.Zou, Lightweight polyimide-derived carbon foams with anisotropic porous structures prepared by microwave-assisted foaming and carbonization for thermal insulation and EMIshielding applications, Journal of Materials Chemistry C 11(39)(2023)(13446-13458), however, its mechanical properties cannot meet the needs of practical applications.
[0004] Therefore, it is necessary to develop a polyimide-based carbon foam that has both high mechanical strength and excellent high-temperature thermal insulation properties, which is of great significance in the fields of aerospace, rocket propulsion systems, and thermal protection of high-temperature industrial equipment. Summary of the invention
[0005] The object of the present invention is to provide a lightweight polyimide-based carbon foam having excellent mechanical strength and high-temperature heat insulation performance, and a preparation method and use thereof.
[0006] The present invention provides a polyimide-based carbon foam, wherein the polyimide-based carbon foam is obtained by reacting an aromatic dianhydride monomer and an aromatic diamine monomer as raw materials to obtain a polyimide precursor, and then foaming, imidizing, and carbonizing the polyimide precursor;
[0007] The molar ratio of the aromatic dianhydride monomer to the aromatic diamine monomer is (1-100):(1-100).
[0008] Furthermore, the molar ratio of the aromatic dianhydride monomer to the aromatic diamine monomer is (1-100):50, preferably 1:1.
[0009] Further, the aromatic dianhydride monomer is selected from any one or more of (3,3',4,4'-benzophenonetetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-oxydiphthalic anhydride);
[0010] and / or the aromatic diamine monomer is selected from any one or more of (4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diaminodiphenyl sulfone);
[0011] Preferably, the aromatic dianhydride monomer is 3,3',4,4'-benzophenonetetracarboxylic dianhydride; and / or the aromatic diamine monomer is 4,4'-diaminodiphenylmethane.
[0012] Furthermore, the reaction includes the following steps: 1) adding a solvent and a ring-opening catalyst to an aromatic dianhydride monomer to obtain an aromatic diacid diester solution; 2) adding an aromatic diamine monomer, an imidization catalyst, and a surfactant to the aromatic diacid diester solution to react, and concentrating under reduced pressure to obtain a product with a solvent content of 10-20wt%, and then crushing and screening to obtain a polyimide precursor with a particle size of 0.05-0.6mm.
[0013] Furthermore, the solvent is a mixture of an alcohol solvent and an ether solvent, the ring-opening catalyst is dimethylimidazole, the imidization catalyst is isoquinoline, and the surfactant is silicone oil DC193; the ratio of the aromatic diamine monomer, the imidization catalyst, and the surfactant is (0.1-4) mol: (0.1-50) mmol: (0.1-5) g;
[0014] The reaction conditions of step 1) are to react at 50-70°C for 0.5-2h under nitrogen or inert gas protection; the reaction conditions of step 2) are to react at 65-85°C for 2-4h;
[0015] Preferably, the alcohol solvent is any one or more of methanol, ethanol, propanol, and isopropanol, and the ether solvent is tetrahydrofuran; the ratio of the aromatic diamine monomer, the imidization catalyst, and the surfactant is (0.3-0.5) mol: (10-30) mmol: (1-2) g.
[0016] Furthermore, the ratio of the aromatic diamine monomer, the imidization catalyst and the surfactant is 0.4 mol:20 mmol:1.04 g.
[0017] Further, the solvent content of the product is 14-17wt%;
[0018] And / or the particle size of the foamed polyimide precursor is 0.1-0.4 mm. Preferably, the particle size of the foamed polyimide precursor is greater than or equal to 0.1 mm and less than 0.2 mm, greater than or equal to 0.2 mm and less than 0.3 mm, or greater than or equal to 0.3 mm and less than or equal to 0.4 mm.
[0019] Furthermore, the foaming condition is to maintain at 120-150° C. for 12-18 min, preferably at 130° C. for 15 min; the imidization condition is to maintain at 250-350° C. for 1-3 h, preferably at 300° C. for 2 h.
[0020] Further, the carbonization condition is carbonization at 600-1600°C for 1-5 hours under nitrogen or inert gas protection, preferably carbonization at 800°C-1400°C for 2-4 hours, preferably carbonization at 800°C-1400°C for 3 hours.
[0021] The present invention also provides a method for preparing the polyimide-based carbon foam. The polyimide-based carbon foam is obtained by reacting aromatic dianhydride monomers and aromatic diamine monomers as raw materials to obtain a polyimide precursor, and then foaming, imidizing and carbonizing the polyimide precursor.
[0022] The present invention also provides a use of the above-mentioned polyimide-based carbon foam in preparing structural materials for use in the fields of aerospace, rocket propulsion systems, and thermal protection of high-temperature industrial equipment.
[0023] The present invention provides a lightweight polyimide-based carbon foam with excellent mechanical strength and high-temperature thermal insulation performance. The present invention copolymerizes aromatic dianhydride and aromatic diamine to prepare polyimide precursor salt PEAS salt, then selects PEAS salts of different particle sizes to obtain imidized foam through microsphere foaming and thermal imidization, and then obtains the polyimide-based carbon foam through high-temperature carbonization. The preparation process of the present invention is simple and easy to operate. The polyimide-based carbon foam has low density, high compression strength, and low thermal conductivity, can be used at high temperatures, and has excellent comprehensive performance. The carbon foam of the present invention can be used as a high-temperature thermal insulation material in the fields of aerospace, rocket propulsion systems, and thermal protection of high-temperature industrial equipment, and has broad application prospects.
[0024] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0025] The following is a further detailed description of the above contents of the present invention through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies implemented based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 XRD and Raman curves of carbon foam treated at different carbonization temperatures.
[0027] Figure 2 The apparent morphology of PIF-1 under different temperature conditions.
[0028] Figure 3 Changes in mass loss rate, volume shrinkage rate, density and pore size of foams treated with different carbonization temperatures.
[0029] Figure 4 Cell morphology and size distribution of PIF foam and carbon foam with different cell sizes.
[0030] Figure 5 Compressive stress-strain curves of foam materials and carbon foam and compressive strength diagram of carbon foam.
[0031] Figure 6 Plots of thermal conductivity and thermal diffusivity of carbon foams treated at different temperatures. DETAILED DESCRIPTION
[0032] The raw materials and equipment used in the present invention are all known products, which are obtained by purchasing commercially available products.
[0033] BTDA: 3,3',4,4'-Benzophenone tetracarboxylic dianhydride (BTDA): CAS number: 2421-28-5
[0034] Example 1: Preparation of polyimide-based carbon foam CPIF of the present invention
[0035] 1. Preparation of polyimide foam (PIF) with different cell sizes
[0036] (1) Preparation of precursor polyester ammonium salt (PEAS):
[0037] Weigh 0.40 mol of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 1.40 mol of methanol (CH 3OH), 1.60 mol of tetrahydrofuran (THF) and 5 mmol of dimethylimidazole (2-MI) were added into a three-necked flask and stirred in an oil bath at 62 °C for 1 h under nitrogen atmosphere. The color of the system solution gradually changed from a milky white liquid to a light yellow clear solution to obtain a clear aromatic diacid diester solution.
[0038] 0.40 mol of 4,4'-diaminodiphenylmethane (MDA), 20 mmol of isoquinoline and 1.04 g of surfactant DC-193 were added to the aromatic diacid diester solution in sequence, and the temperature of the oil bath pot was raised to 70-72°C for reaction for 3 hours to obtain a reddish brown transparent PEAS solution. Part of the solvent was removed at 65°C and -0.6 MPa to obtain PEAS salt, and the solvent content in the final PEAS salt was 14-17 wt%. The PEAS salt containing 14-17 wt% of solvent was crushed and sieved to obtain PEAS salt particles with particle sizes of greater than or equal to 0.1 mm and less than 0.2 mm, greater than or equal to 0.2 mm and less than 0.3 mm, and greater than or equal to 0.3 mm and less than 0.4 mm;
[0039] (2) Preparation of PIF foams with different cell sizes:
[0040] The above-mentioned PEAS salt particles with different particle sizes were placed in a 130°C forced air oven for 15 minutes to obtain light yellow non-imidized hollow microspheres, and then the hollow microspheres were transferred and filled into a mold, and kept at 300°C for 2 hours to complete the imidization. After the mold was cooled to room temperature, the PIF foam was taken out, and the foams were named PIF-1, PIF-2 and PIF-3 according to the PEAS particle size greater than or equal to 0.1 mm and less than 0.2 mm, greater than or equal to 0.2 mm and less than 0.3 mm, and greater than or equal to 0.3 mm and less than 0.4 mm.
[0041] 2. Preparation of polyimide-based carbon foam CPIF
[0042] The PIF foam obtained in step 1 was placed in a tube furnace and carbonized at 800°C, 1100°C and 1400°C under a nitrogen atmosphere for 3 h to obtain a polyimide-based carbon foam (CPIF), which was named C 800 -PIF, C 1100 -PIF and C 1400 -PIF;C 800 -PIF-1 refers to the carbon foam sample obtained by PIF-1 at 800°C, and so on. The specific naming method is shown in Table 1.
[0043] CPIF-1, CPIF-2, and CPIF-3 represent carbon foams obtained by high-temperature carbonization of PIF-1, PIF-2, and PIF-3, respectively.
[0044] Table 1 CPIF nomenclature
[0045]
[0046]
[0047] The beneficial effects of the present invention are demonstrated by experimental examples below.
[0048] Experimental Example 1: Structural Characterization of the Polyimide-based Carbon Foam of the Present Invention
[0049] 1. Experimental Methods
[0050] The CPIF carbon foam material of the present invention is subjected to X-ray diffraction analysis (XRD) and Raman spectroscopy analysis (Raman)
[0051] 2. Experimental Results
[0052] X-ray diffraction analysis of PIF-1 and CPIF-1 Figure 1 As shown in (a), PIF-1 has broad peaks near 20° and 40°, corresponding to the amorphous structure of the PI chain and the π-π stacking between aromatic rings or imide rings, respectively. The XRD curves of CPIF-1 both have 002 and 101 peaks of carbon structure, where the 002 peak represents the peak of the amorphous carbon structure and the 101 peak represents the peak of graphitized carbon. As the carbonization temperature gradually increases, the 101 peak of graphitized carbon increases, while the 002 peak weakens, indicating that increasing temperature is more conducive to the formation of graphitized structure.
[0053] Figure 1 (b) shows the Raman curve of CPIF-1. The yellow color of uncarbonized PIF-1 interferes with the test signal, so no valid data can be measured. The Raman curve of CPIF-1 is at 1590cm -1 and 1345cm -1 The G band and D band of carbon materials belong to the graphitized structure and amorphous structure of carbon, respectively. D / I G The ratio of I is used to characterize the degree of graphitization of the carbon structure. As the carbonization temperature increases, D / I G The value of decreases from 1.050 to 1.004, indicating that the degree of graphitization of the carbon layer is gradually increasing.
[0054] In summary, the carbonization temperature is between 800° C. and 1400° C., and the graphitization degree of the polyimide-based carbon foam prepared by the present invention gradually increases with the increase of the carbonization temperature, and the higher the carbonization temperature, the more conducive it is to the formation of an ordered carbon structure.
[0055] Experimental Example 2: Microscopic Morphology of the Polyimide-Based Carbon Foam of the Present Invention
[0056] 1. Experimental Methods
[0057] The microstructure of polyimide-based carbon foam was observed using a scanning electron microscope, and the size of the foam was measured using Nano Measurer software. The mass, density, and volume of PIF-1 before and after carbonization were measured, and the mass loss rate, density, and volume shrinkage were calculated.
[0058] 2. Experimental Results
[0059] PIF-1, C 800 -PIF-1, C 1100 -PIF-1 and C 1400 -PIF-1's appearance is as follows Figure 2 As shown in the figure, it can be seen that the appearance of PIF-1 before and after carbonization is basically the same, and the color changes greatly. The uncarbonized PIF-1 foam is brown-yellow, and after high-temperature carbonization, it is black as a whole. However, the carbonized foam shrinks to a certain extent.
[0060] like Figure 3 As shown in Figure 2, at 800°C, the mass loss of PIF-1 foam material is 41.4%, and the volume shrinkage is 46-48%. When the temperature rises to 1400°C, the mass loss of the foam is 45.0%, and the volume shrinkage is 45-49%. The mass loss and volume shrinkage are mainly attributed to the CO, CH 4 and N 2 Nevertheless, PIF-1 was carbonized at high temperature to obtain CPIF-1, and compared with PIF-1, the front and top surfaces of CPIF-1 were intact and had no major defects.
[0061] The density of each foam material is Figure 3 As shown, it can be seen that among PIF-1, PIF-2 and PIF-3, PIF-3 has the lowest density. The density of carbonized foams obtained by carbonizing PIF-1 and PIF-2 at different temperatures shows a trend of first decreasing and then increasing. 800 -PIF-3 has the lowest density of all foam materials (including carbon foam).
[0062] PIF-1, C 800 -PIF-1, C 1100 -PIF-1 and C 1400 -The SEM results of PIF-1 are as follows Figure 4As shown in the figure, it can be seen that the pores of PIF-1 are very uniform, and the gaps between the pore walls are relatively small. After high-temperature carbonization, the interaction between the pores is weakened, and with the increase of carbonization temperature, the internal defects of the carbonized foam tend to increase. This is mainly because the PI chain segments produce CO and N during the pyrolysis process during the carbonization process. 2 and CH 4 , causing the cells to shrink and increasing the gaps between the cells.
[0063] The average pore size of PIF-1, PIF-2 and PIF-3 increases with the increase of PEAS salt particle size, which are 264, 392 and 650 μm, respectively. Meanwhile, the average pore size of the foam decreases with the increase of temperature. 1400 -PIF-1, C 1400 -PIF-2 and C 1400 -PIF-3 average cell sizes were 208, 333 and 534 μm, respectively. 800 -PIF-1, C 1100 -PIF-1 and C 1400 -PIF-1 carbon foam has no defects in its cell walls and is basically closed, which indicates that carbonizing PIF is an effective way to obtain carbon foam with intact and uniform internal morphology.
[0064] Experimental Example 3: Performance Characterization of the Polyimide-Based Carbon Foam of the Present Invention
[0065] 1. Experimental Methods
[0066] (I) Compression performance test of carbon foam of the present invention
[0067] Determine the compressive stress strain and compressive strength of PIF foam and carbon foam. The compression performance test of PIF foam and carbon foam refers to the national standard GB / T 1041-1992. The foam size is a cylinder with a diameter of 35mm and a height of 20mm or a rectangular block with a length of 30mm, a width of 30mm and a height of 20mm. The compression rate is set to 2mm·min -1 , the strain is 50%.
[0068] (II) Thermal conductivity and thermal diffusivity test of carbon foam
[0069] The thermal conductivity and thermal diffusivity of different carbon foams were measured respectively. The thermal conductivity test method at room temperature is as follows: The room temperature thermal conductivity is measured using a Hot Disk TPS2500S thermal constant analyzer. The test sample is made into a cuboid with a length of 30 mm, a width of 30 mm and a height of 20 mm.
[0070] High temperature (500℃ and 1000℃) thermal conductivity test method: The high temperature thermal conductivity of carbon foam is tested according to the reference standard ISO22007-2 using the transient flat plate heat source method. The hot plate sensor is placed between two pieces of carbon foam and the thermal conductivity of the two carbon foams is collected at the same time. The thermal conductivity obtained is the average value of the two samples.
[0071] 2. Experimental Results
[0072] (I) Compression performance test results of carbon foam of the present invention
[0073] The present invention first defines the compressive strength of the foam material and the carbon foam. The stress corresponding to 10% strain of the foam material is considered to be the compressive strength. Figure 5 As shown in the black stress-strain curve in (a), for carbon foam, the stress fluctuates greatly during the compression process, indicating that there are many defects inside the carbon foam.
[0074] Based on this, the compressive strength of PIF-1, PIF-2 and PIF-3 under different carbonization temperature conditions is shown in Figure 2. Figure 5 As shown in (b), the compressive strengths of PIF-1, PIF-2 and PIF-3 are 0.56, 0.47 and 0.24 MPa respectively. However, the compressive strength of carbon foam obtained by carbonizing PIF foam at 800℃ is lower than that of PIF foam. 800 -PIF-1 has a lower compressive strength than PIF-1. PIF foams with different foam sizes were carbonized at 800, 1100 and 1400℃, and the change pattern of the compressive strength of carbon foams was basically similar, that is, the compressive strength showed a trend of first decreasing, then increasing and then decreasing. In addition, the strength of PIF-1 after carbonization was still higher than that of PIF-2 and PIF-3, among which C 1100- The compressive strength of PIF-1 reaches the highest value of 0.74MPa.
[0075] The experimental results show that the compression strengths of PIF-1, PIF-2 and PIF-3 foams obtained with different PEAS salt particle sizes are different, among which PIF-1 has the highest compression strength. The compression strengths of carbon foams obtained by carbonizing PIF-1, PIF-2 and PIF-3 at different temperatures first decrease, then increase and then decrease with the carbonization temperature. The unexpected C 1100- The compressive strength of PIF-1 is the most significant, reaching 0.74MPa.
[0076] (II) Test results of thermal conductivity and thermal diffusivity of carbon foam
[0077] The thermal diffusion coefficient is used to measure the ability of temperature to reach equilibrium. The smaller the thermal diffusion coefficient, the slower the heat diffusion. At room temperature, the thermal conductivity of PIF-1, PIF-2 and PIF-3 under different carbonization temperature conditions is as follows: Figure 6As shown in (a), the thermal conductivities of PIF-1, PIF-2, and PIF-3 are 0.056, 0.051, and 0.048 W·m, respectively. -1 K -1 , indicating that the foam material has good thermal insulation ability. It can be seen that under normal temperature, the thermal conductivity of PIF-3 is the lowest.
[0078] At room temperature, when the carbonization temperature of PIF-1 increases from 800℃ to 1400℃, the thermal conductivity increases from 0.126W·m -1 K -1 Increased to 0.244W·m -1 K -1 , thermal diffusion coefficient from 0.38mm 2 ·s -1 Increase to 0.50mm 2 ·s -1 .
[0079] Carbon foam C 800 -PIF-3 has the lowest room temperature thermal conductivity, only 0.083 W·m -1 K -1 Therefore, the carbon foam C obtained by carbonization at 800℃ 800 The thermal conductivity of -PIF at 500℃ and 1000℃ was characterized, and the specific results are shown in Table 2.
[0080] Table 2C 800 -Thermal conductivity and thermal diffusivity of PIF at 500℃ and 1000℃
[0081]
[0082] From Table 2, we can see that C 800 -PIF-1, C 800 -PIF-2 and C 800 -The thermal conductivity of PIF-3 at 500℃ and 1000℃ is low and the difference is not big, which is maintained at 0.200~0.280W·m -1 K -1 The thermal diffusion coefficients of carbon foams prepared with different particle sizes vary significantly. 800 -PIF-3 diffusion coefficient is much lower than C 800 -PIF-1 and C 800 -PIF-2, C 800 -PIF-3 has the best thermal insulation performance.
[0083] The present invention provides a lightweight polyimide-based carbon foam with excellent mechanical strength and high-temperature heat insulation performance. The present invention copolymerizes aromatic dianhydride and aromatic diamine to prepare polyimide precursor salt PEAS salt, then selects PEAS salts of different particle sizes to foam microspheres, thermally imidize to obtain imidized foam, and then high-temperature carbonizes to obtain the polyimide-based carbon foam. The preparation process of the present invention is simple and easy to operate. The polyimide-based carbon foam has low density, high compression strength, and low thermal conductivity, can be used at high temperatures, and has excellent comprehensive performance, wherein C 800 -The thermal conductivity of PIF-3 at room temperature is only 0.083 W·m -1 K -1 , at 500℃ and 1000℃C 800 -PIF-3 thermal diffusivity is less than 1mm 2 ·s -1 . C 800 -PIF-1, C 800 -PIF-2 and C 800 -The thermal conductivity of PIF-3 at 500℃ and 1000℃ is maintained at 0.200~0.280W·m -1 K -1 In the range, C 1100 - The compression strength of PIF-1 is the maximum value of 0.74 MPa among all carbon foams. The carbon foam of the present invention can be used as a high-temperature thermal insulation material in the fields of aerospace, rocket propulsion system, thermal protection of high-temperature industrial equipment, etc., and has good application prospects.
Claims
1. A polyimide-based carbon foam, characterized in that: The polyimide-based carbon foam is obtained by reacting aromatic dianhydride monomers and aromatic diamine monomers as raw materials to obtain a polyimide precursor, and then foaming, imidizing, and carbonizing the polyimide precursor; The molar ratio of the aromatic dianhydride monomer to the aromatic diamine monomer is (1-100):(1-100).
2. The polyimide-based carbon foam according to claim 1, characterized in that: The molar ratio of the aromatic dianhydride monomer to the aromatic diamine monomer is (1-100):50, preferably 1:
1.
3. The polyimide-based carbon foam according to claim 1 or 2, characterized in that: The aromatic dianhydride monomer is selected from any one or more of (3,3',4,4'-benzophenonetetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-oxydiphthalic anhydride); and / or the aromatic diamine monomer is selected from any one or more of (4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diaminodiphenyl sulfone); Preferably, the aromatic dianhydride monomer is 3,3',4,4'-benzophenonetetracarboxylic dianhydride; and / or the aromatic diamine monomer is 4,4'-diaminodiphenylmethane.
4. The polyimide-based carbon foam according to claim 1, characterized in that: The reaction comprises the following steps: 1) adding a solvent and a ring-opening catalyst to an aromatic dianhydride monomer to react to obtain an aromatic diacid diester solution; 2) adding an aromatic diamine monomer, an imidization catalyst and a surfactant to the aromatic diacid diester solution to react, and concentrating under reduced pressure to obtain a product with a solvent content of 10-20wt%, and then crushing and screening to obtain a polyimide precursor with a particle size of 0.05-0.6mm.
5. The polyimide-based carbon foam according to claim 4, characterized in that: The solvent is a mixture of an alcohol solvent and an ether solvent, the ring-opening catalyst is dimethylimidazole, the imidization catalyst is isoquinoline, and the surfactant is silicone oil DC193; the ratio of the aromatic diamine monomer, the imidization catalyst, and the surfactant is (0.1-4) mol: (0.1-50) mmol: (0.1-5) g; The reaction conditions of step 1) are to react at 50-70°C for 0.5-2h under nitrogen or inert gas protection; the reaction conditions of step 2) are to react at 65-85°C for 2-4h; Preferably, the alcohol solvent is any one or more of methanol, ethanol, propanol, and isopropanol, and the ether solvent is tetrahydrofuran; the ratio of the aromatic diamine monomer, the imidization catalyst, and the surfactant is (0.3-0.5) mol: (10-30) mmol: (1-2) g; Furthermore, the ratio of the aromatic diamine monomer, the imidization catalyst and the surfactant is 0.4 mol:20 mmol:1.04 g.
6. The polyimide-based carbon foam according to claims 1-5, characterized in that: The solvent content of the product is 14-17 wt %; And / or the particle size of the foamed polyimide precursor is 0.1-0.4 mm. Preferably, the particle size of the foamed polyimide precursor is greater than or equal to 0.1 mm and less than 0.2 mm, greater than or equal to 0.2 mm and less than 0.3 mm, or greater than or equal to 0.3 mm and less than or equal to 0.4 mm.
7. The polyimide-based carbon foam according to claims 1-5, characterized in that: The foaming condition is to keep at 120-150° C. for 12-18 minutes, preferably at 130° C. for 15 minutes; the imidization condition is to keep at 250-350° C. for 1-3 hours, preferably at 300° C. for 2 hours.
8. The polyimide-based carbon foam according to claims 1-7, characterized in that: The carbonization conditions are: carbonization at 600-1600° C. for 1-5 hours under nitrogen or inert gas protection, preferably carbonization at 800° C.-1400° C. for 2-4 hours, preferably carbonization at 800° C.-1400° C. for 3 hours.
9. A method for preparing the polyimide-based carbon foam according to claims 1-8, characterized in that: The method comprises the following steps: the polyimide-based carbon foam is obtained by reacting aromatic dianhydride monomers and aromatic diamine monomers as raw materials to obtain a polyimide precursor, and then foaming, imidizing and carbonizing the polyimide precursor.
10. Use of the polyimide-based carbon foam according to claims 1-8 in the preparation of structural materials for use in the fields of aerospace, rocket propulsion systems, equipment and thermal protection of high-temperature industrial equipment.
Citation Information
Patent Citations
Polyimide foam, and preparation method and application thereof
CN109880096A
High-performance high-temperature-resistant thermal insulation polyimide foam and application thereof
CN116199884A
Light polyimide-based carbon foam as well as preparation method and application thereof
CN117049507A
Anisotropic high-temperature heat-insulation flame-retardant polyimide foam as well as preparation method and application thereof
CN118027406A
Carbon porous body and its manufacturing process
JP2005041748A