Preparation method of nitrogen-doped reduced graphene oxide / zinc ferrite nitrogen-doped carbon nano composite wave-absorbing material

Nitrogen-doped reduced graphene oxide/zinc ferrite@nitrogen-doped carbon nanocomposite was prepared through solvothermal, autopolymerization, carbonization and hydrothermal steps, which solved the problems of high density and low absorption intensity of traditional absorbing materials and achieved It has low filling ratio, high absorption intensity and wide-band electromagnetic wave absorption effect, and is suitable for the treatment of electromagnetic wave pollution.

CN118851162APending Publication Date: 2024-10-29ANHUI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410834148.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Traditional electromagnetic wave absorbing materials have high density, low absorption intensity, and narrow absorption band. They cannot meet the requirements of new wave absorbing materials with light weight, wide absorption band, and strong absorption capacity. They are especially deficient in the problem of electromagnetic pollution.

Method used

Zinc ferrite was synthesized through solvothermal reaction, ZnFe2O4@NC composite was obtained by dopamine self-polymerization and carbonization process, and nitrogen-doped reduced graphene oxide/zinc ferrite@nitrogen-doped carbon (NRGO/ ZnFe2O4@NC) nanocomposite material achieves a uniform load core-shell structure and multiple heterogeneous interfaces of the composite material, and adjusts the composition and thickness to achieve electromagnetic wave absorption in different bands.

Benefits of technology

The prepared NRGO/ZnFe2O4@NC nanocomposite absorbing material has a low filling ratio, high absorption intensity and wide frequency band, and can cover the entire Ku band and part of the X band. The preparation process is green and pollution-free, and the absorption intensity can reach -61.1dB, which is effective. The absorption bandwidth reaches 7.2GHz.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851162A_ABST
    Figure CN118851162A_ABST
Patent Text Reader

Abstract

The invention discloses a nitrogen-doped reduced graphene oxide / zinc ferrite nitrogen-doped carbon nano composite wave-absorbing material and a preparation method thereof. Firstly, ferric chloride hexahydrate and zinc chloride are used as metal salt precursors, and zinc ferrite is synthesized through solvothermal reaction; then, self-polymerizing dopamine on the surface of the zinc ferrite to obtain a zinc ferrite and polydopamine compound with a core-shell structure, and further carbonizing to obtain a zinc ferrite and nitrogen-doped carbon compound; and finally, synthesizing the nitrogen-doped reduced graphene oxide / zinc ferrite nitrogen-doped carbon nano composite material by taking graphene oxide as a template and adopting a hydrothermal method. The preparation method is green and environment-friendly, and no toxic and harmful by-products are generated. The prepared nano composite material is formed by uniformly loading core-shell structure zinc ferrite and nitrogen-doped carbon microspheres on the surface of a nitrogen-doped reduced graphene oxide sheet. The ternary nano composite material not only has the characteristics of low packing ratio and high absorption strength, but also can realize broadband absorption of the whole Ku wave band and part of X wave band. In addition, electromagnetic waves of different wave bands can be effectively absorbed by adjusting the composition and thickness of the composite material. Therefore, the prepared nitrogen-doped reduced graphene oxide / zinc ferrite nitrogen-doped carbon nano composite material has important application value in the field of electromagnetic wave absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electromagnetic wave absorbing materials, and specifically relates to a nitrogen-doped reduced graphene oxide / zinc ferrite@nitrogen-doped carbon nanocomposite absorbing material and a preparation method thereof. Technical Background

[0002] Due to the excessive use of electronic devices, serious electromagnetic radiation pollution has been caused, making electromagnetic wave absorbing materials (absorbent materials for short) gradually become a research hotspot in the field of functional materials. Traditional absorbing materials usually have disadvantages such as high density, low absorption intensity, and narrow absorption bandwidth, which cannot meet the requirements of new absorbing materials with light weight, wide absorption bandwidth, and strong absorption capacity. Therefore, it is urgent to develop new absorbing materials with excellent comprehensive absorbing performance to solve the problem of electromagnetic pollution.

[0003] Reduced graphene oxide (RGO) is a typical two-dimensional carbon nanomaterial, which is generally prepared from natural graphite by chemical oxidation-reduction method. The RGO sheets prepared by this method have a large number of defects on the surface, and the surface and edges carry abundant oxygen-containing functional groups, which not only helps to improve the electromagnetic impedance matching characteristics of RGO; but also, under the alternating electromagnetic field, the defects and functional groups remaining on the surface of RGO will cause defect polarization and electronic dipole polarization relaxation, making RGO have stronger dielectric loss and wave absorption ability compared with graphite, carbon nanotubes, etc. Therefore, RGO has good application prospects in the field of wave absorbing materials.

[0004] Although RGO has high electrical conductivity, a single dielectric loss mechanism will lead to unsatisfactory wave absorption performance. Therefore, RGO is compounded with magnetic materials to prepare RGO-based composite materials. By introducing magnetic loss and enhancing dielectric loss, impedance matching can be optimized and the attenuation loss capability can be improved. Zinc ferrite (ZnFe2O4), as a typical spinel ferrite, has received extensive attention in the field of wave absorbing materials in recent years due to its simple synthesis method, low cost, good dielectric loss and magnetic loss characteristics.

[0005] Polydopamine (PDA) is a polymer material formed by the self-polymerization of dopamine (DA). Nitrogen-doped carbon (NC) can be obtained after carbonization treatment. Coating PDA on the surface of magnetic particles can effectively prevent the oxidation of magnetic particles and produce abundant heterogeneous interfaces with magnetic particles, thereby improving the wave absorption performance. ZnFe2O4 is easily oxidized in the air or corroded under acidic conditions, thereby reducing the magnetic loss performance, thus limiting its application in oxidative or corrosive environments. After coating the surface of ZnFe2O4 particles with PDA and then carbonizing them, zinc ferrite @ nitrogen-doped carbon (ZnFe2O4@NC) composites can be obtained, thereby improving the antioxidant and corrosion resistance of ZnFe2O4. In addition, combining RGO with ZnFe2O4@NC can achieve a synergistic effect between different components of RGO, ZnFe2O4 and NC. The abundant heterogeneous interfaces formed between RGO and NC, and ZnFe2O4 and NC can form interface polarization, which is helpful for the attenuation of electromagnetic waves. However, there are few reports on the composite of NC-coated ZnFe2O4 and RGO to prepare nitrogen-doped reduced graphene oxide / zinc ferrite@nitrogen-doped carbon (NRGO / ZnFe2O4@NC) nanocomposite absorbers.

[0006] The present invention first synthesizes zinc ferrite by solvent thermal reaction, then obtains ZnFe2O4@NC composite by dopamine self-polymerization and carbonization process, and finally prepares NRGO / ZnFe2O4@NC nanocomposite by hydrothermal method. By adjusting the composition and thickness of the composite material, effective absorption of electromagnetic waves of different bands can be achieved. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a NRGO / ZnFe2O4@NC nanocomposite absorbing material. The nanocomposite material not only has the characteristics of low filling ratio and high absorption intensity, but also can achieve broadband absorption of the entire Ku band and part of the X band, and its preparation process is green and pollution-free.

[0008] The present invention is achieved through the following technical solutions:

[0009] A NRGO / ZnFe2O4@NC nanocomposite wave absorbing material, wherein the composite wave absorbing material is composed of ZnFe2O4@NC microspheres with a core-shell structure uniformly loaded on the surface of a NRGO sheet.

[0010] A method for preparing a NRGO / ZnFe2O4@NC nanocomposite wave absorbing material, the steps of which are as follows:

[0011] (1) Add 5 mmol of ferric chloride hexahydrate and 2.5 mmol of zinc chloride to 40 mL of ethylene glycol solution and stir vigorously to completely dissolve them;

[0012] (2) Add 3.6 g of sodium acetate to the above solution and stir for 1 h, then add 2 g of polyethylene glycol-6000 and stir in a 55°C oil bath for 2 h;

[0013] (3) The above solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel reactor and subjected to solvothermal reaction at 200 °C for 8 h;

[0014] (4) After the reaction is completed, the mixture is cooled to room temperature, washed with anhydrous ethanol and deionized water until the pH is neutral, and the product is collected by magnetic separation;

[0015] (5) pre-freezing the product collected in step (4) for 12 hours and then freeze-drying it in vacuum for 36 hours to obtain ZnFe2O4;

[0016] (6) Add 0.1212 g of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, then add 100 mg of ZnFe2O4 obtained in step (5), and sonicate for 1 h until the mixture is evenly dispersed;

[0017] (7) Add 0.1 g DA to step (6), stir at room temperature for 24 h, and wash the product with deionized water until the pH is neutral;

[0018] (8) The product collected in step (7) was pre-frozen for 12 hours and then vacuum freeze-dried for 36 hours to obtain ZnFe2O4@PDA;

[0019] (9) heating the collected ZnFe2O4@PDA obtained in step (8) to 500°C at a heating rate of 2°C / min under argon and keeping the temperature for 2 h to obtain ZnFe2O4@NC;

[0020] (10) In a 150 mL beaker, 60 mL of deionized water and 60 mg of multilayer graphene oxide were added in sequence and ultrasonicated for 30 min to form a graphene oxide (GO) dispersion with a concentration of 1 mg / mL;

[0021] (11) Add 60 mg of ZnFe2O4@NC obtained in step (8) to the GO dispersion obtained in step (10), and after ultrasonic and mechanical stirring for 1 h each, add 180 μL of ethylenediamine and stir vigorously for 2 h;

[0022] (12) The above dispersion was transferred to a 100 mL reactor and subjected to hydrothermal reaction at 120 °C for 12 h;

[0023] (13) After the reaction, the mixture was naturally cooled to room temperature, washed with deionized water until the pH was neutral, and the product was collected by magnetic separation. After pre-freezing for 12 h, it was vacuum freeze-dried for 36 h to obtain NRGO / ZnFe2O4@NC nanocomposite materials.

[0024] Compared with the prior art, the beneficial technical effects of the present invention are embodied in the following aspects:

[0025] 1. The NRGO / ZnFe2O4@NC nanocomposite absorbing material prepared by the present invention is green and safe, and does not produce any toxic or harmful substances.

[0026] 2. The NRGO / ZnFe2O4@NC nanocomposite absorber material is composed of ZnFe2O4@NC microspheres with core-shell structure uniformly loaded on the surface of NRGO thin sheets.

[0027] 3. NRGO / ZnFe2O4@NC nanocomposite absorbers have excellent absorbing properties, with low filling ratio, high absorption intensity, and wide absorption bandwidth. At a thickness of 3.06mm, the absorption intensity of the composite absorber can reach -61.1dB, and the effective absorption bandwidth can reach 6GHz, covering the entire Ku band; at a thickness of 2.61mm, the widest effective absorption bandwidth is 7.2GHz, covering the entire Ku band and part of the X band.

[0028] 4. The NRGO / ZnFe2O4@NC nanocomposite absorbing material prepared by the present invention can realize the effective absorption of electromagnetic waves by the composite material through nitrogen doping, core-shell structure and multiple heterogeneous interface structure design, combined with the synergistic effect of physical mechanisms such as dielectric loss, conductive loss and magnetic loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is the X-ray diffraction (XRD) spectra of the products in Examples 1, 2, and 3;

[0030] Figure 2 is the Raman spectra of the products in Examples 1, 2, and 3;

[0031] Figure 3 is the X-ray photoelectron spectroscopy (XPS) spectrum of the product S3 in Example 3;

[0032] Figure 4 are scanning electron microscope (SEM) images of the products in Examples 1, 2, and 3 and a transmission electron microscope (TEM) image of the product S3 in Example 3;

[0033] Figure 5 is the curve of reflection loss versus frequency of product S1 in Example 1;

[0034] Figure 6 is the curve of reflection loss versus frequency of product S2 in Example 2;

[0035] Figure 7 is the curve of reflection loss versus frequency of product S3 in Example 3;

[0036] Figure 8 is the curve of eddy current coefficient of the products in Examples 1, 2 and 3 changing with frequency;

[0037] Fig. 9 It is the attenuation constant variation curve of the products in Examples 1, 2 and 3 as a function of frequency. Specific implementation methods

[0039] The present invention will now be further described with reference to the embodiments and accompanying drawings:

[0040] Example 1

[0041] (1) Add 5 mmol of ferric chloride hexahydrate and 2.5 mmol of zinc chloride to 40 mL of ethylene glycol solution and stir vigorously to completely dissolve them;

[0042] (2) Add 3.6 g of sodium acetate to the above solution and stir for 1 h, then add 2 g of polyethylene glycol-6000 and stir in a 55°C oil bath for 2 h;

[0043] (3) The above solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel reactor and subjected to solvothermal reaction at 200 °C for 8 h;

[0044] (4) After the reaction is completed, the mixture is cooled to room temperature, washed with anhydrous ethanol and deionized water until the pH is neutral, and the product is collected by magnetic separation;

[0045] (5) pre-freezing the product collected in step (4) for 12 hours and then freeze-drying it in vacuum for 36 hours to obtain ZnFe2O4;

[0046] (6) Add 0.1212 g of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, then add 100 mg of ZnFe2O4 obtained in step (5), and sonicate for 1 h until the mixture is evenly dispersed;

[0047] (7) Add 0.1 g DA to step (6), stir at room temperature for 24 h, and wash the product with deionized water until the pH is neutral;

[0048] (8) The product collected in step (7) was pre-frozen for 12 hours and then vacuum freeze-dried for 36 hours to obtain ZnFe2O4@PDA;

[0049] (9) The collected ZnFe2O4@PDA obtained in step (8) was heated to 500°C at a heating rate of 2°C / min under argon and kept at this temperature for 2 h to obtain ZnFe2O4@NC, which was labeled as S1.

[0050] The XRD spectrum of the product of Example 1 is as follows Figure 1As shown. The positions at 2θ=18.2°, 29.9°, 35.3°, 36.9°, 42.8°, 46.9°, 53.1°, 56.6° and 62.2° are consistent with the positions corresponding to the (111), (220), (311), (222), (400), (422), (511), (440) and (533) crystal planes of the ZnFe2O4 standard card (JCPDS Card No.22-1012). The Raman spectrum of the product of Example 1 is shown in Figure 2 S1 at 1588cm -1 (G band) and 1345cm -1 There are two obvious diffraction peaks near (D band), I D / I G The SEM image of the product of Example 1 is shown in Figure 4 (a)–(c) show that the surface of the ZnFe2O4 microspheres is tightly wrapped by the NC layer. The powder product in Example 1 was mixed with paraffin wax, and a coaxial sample with an outer diameter of 7 mm, an inner diameter of 3.04 mm, and a thickness of about 2 mm was pressed in a special mold at a filling ratio of 16.5 wt.%. The electromagnetic parameters were tested using a Keysight E5080B vector network analyzer, and the wave absorption performance was calculated. The test frequency range was 2–18 GHz. The reflection loss of sample S1 changes with frequency as shown in the following figure: Figure 5 As shown in FIG. 1 , when the matching thickness is 5 mm, the maximum absorption intensity reaches -0.84 dB at 8.24 GHz. The eddy current coefficient of the product of Example 1 varies with frequency. Figure 8 In the range of 2-4 GHz, the eddy current coefficient increases sharply as the frequency decreases, indicating that the magnetic loss is mainly due to natural resonance; it remains basically unchanged at 14-18 GHz, indicating that the magnetic loss is mainly due to eddy current loss. The attenuation constant of the product of Example 1 varies with frequency. Fig. 9 The larger the value, the stronger the attenuation capability. The attenuation constant of S1 increases gradually with the increase of frequency, and its maximum attenuation constant value is 9.5.

[0051] Example 2

[0052] (1) Add 5 mmol of ferric chloride hexahydrate and 2.5 mmol of zinc chloride to 40 mL of ethylene glycol solution and stir vigorously to completely dissolve them;

[0053] (2) Add 3.6 g of sodium acetate to the above solution and stir for 1 h, then add 2 g of polyethylene glycol-6000 and stir in a 55°C oil bath for 2 h;

[0054] (3) The above solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel reactor and subjected to solvothermal reaction at 200 °C for 8 h;

[0055] (4) After the reaction is completed, the mixture is cooled to room temperature, washed with anhydrous ethanol and deionized water until the pH is neutral, and the product is collected by magnetic separation;

[0056] (5) pre-freezing the product collected in step (4) for 12 hours and then freeze-drying it in vacuum for 36 hours to obtain ZnFe2O4;

[0057] (6) Add 60 mL of deionized water and 60 mg of GO into a 150 mL beaker and sonicate for 30 min to form a GO dispersion with a concentration of 1 mg / mL;

[0058] (7) Add 60 mg of ZnFe2O4 obtained in step (5) to the GO dispersion obtained in step (6), and after ultrasonic and mechanical stirring for 1 h each, add 180 μL of ethylenediamine and stir vigorously for 2 h;

[0059] (8) The above dispersion was transferred to a 100 mL reactor and subjected to hydrothermal reaction at 120 °C for 12 h;

[0060] (9) After the reaction, the mixture was naturally cooled to room temperature, washed with deionized water until the pH was neutral, and the product was collected by magnetic separation. After pre-freezing for 12 h, it was vacuum freeze-dried for 36 h to obtain a NRGO / ZnFe2O4 composite material, which was labeled as S2.

[0061] The XRD spectra of the product of Example 2 are as follows Figure 1 As shown. The positions at 2θ = 18.2°, 29.9°, 35.3°, 36.9°, 42.8°, 46.9°, 53.1°, 56.6° and 62.2° are consistent with the positions corresponding to the (111), (220), (311), (222), (400), (422), (511), (440) and (533) crystal planes of the ZnFe2O4 standard card (JCPDS Card No. 22-1012), and the characteristic peak at 2θ = 24.7° corresponds to the (002) crystal plane of RGO. The Raman spectrum of the product of Example 2 is shown in Figure 2 ,S2 at 1588cm -1 (G band) and 1345cm -1 There are two obvious diffraction peaks near (D band), I D / I G The SEM image of the product of Example 2 is shown in Figure 4(d)–(f) show that ZnFe2O4 microspheres are uniformly attached to the wrinkled NRGO surface. The product in Example 2 was mixed with paraffin wax, and a coaxial sample with an outer diameter of 7 mm, an inner diameter of 3.04 mm, and a thickness of about 2 mm was pressed in a special mold at a filling ratio of 16.5 wt.%. The electromagnetic parameters were tested using a Keysight E5080B vector network analyzer, and the wave absorption performance was calculated. The test frequency range was 2–18 GHz. The reflection loss of sample S2 changes with frequency as shown in the figure. Figure 6 As shown in FIG. 1 , when the matching thickness is 5 mm, the maximum absorption intensity reaches -16.8 dB at 6.88 GHz; when the matching thickness is 2.62 mm, the maximum effective absorption bandwidth is 5 GHz. The eddy current coefficient of the product of Example 2 varies with frequency. Figure 8 In the range of 2-6 GHz, the eddy current coefficient increases sharply as the frequency decreases, indicating that the magnetic loss is mainly due to natural resonance; it remains basically unchanged at 14-18 GHz, indicating that the magnetic loss is mainly due to eddy current loss. The attenuation constant of the product of Example 2 changes with frequency. Fig. 9 The larger the value, the stronger the attenuation capability. The attenuation constant of S2 increases gradually with the increase of frequency, and its maximum attenuation constant value is 139.6.

[0062] Example 3

[0063] (1) Add 5 mmol of ferric chloride hexahydrate and 2.5 mmol of zinc chloride to 40 mL of ethylene glycol solution and stir vigorously to completely dissolve them;

[0064] (2) Add 3.6 g of sodium acetate to the above solution and stir for 1 h, then add 2 g of polyethylene glycol-6000 and stir in a 55°C oil bath for 2 h;

[0065] (3) The above solution was transferred to a 50 mL polytetrafluoroethylene-lined stainless steel reactor and subjected to solvothermal reaction at 200 °C for 8 h;

[0066] (4) After the reaction is completed, the mixture is cooled to room temperature, washed with anhydrous ethanol and deionized water until the pH is neutral, and the product is collected by magnetic separation;

[0067] (5) pre-freezing the product collected in step (4) for 12 hours and then freeze-drying it in vacuum for 36 hours to obtain ZnFe2O4;

[0068] (6) Add 0.1212 g of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, then add 100 mg of ZnFe2O4 obtained in step (5), and sonicate for 1 h until the mixture is evenly dispersed;

[0069] (7) Add 0.1 g DA to step (6), stir at room temperature for 24 h, and wash the product with deionized water until the pH is neutral;

[0070] (8) The product collected in step (7) was pre-frozen for 12 hours and then vacuum freeze-dried for 36 hours to obtain ZnFe2O4@PDA;

[0071] (9) heating the collected ZnFe2O4@PDA obtained in step (8) to 500°C at a heating rate of 2°C / min under argon and keeping the temperature for 2 h to obtain ZnFe2O4@NC;

[0072] (10) In a 150 mL beaker, add 60 mL of deionized water and 60 mg of GO in sequence and sonicate for 30 min to form a GO dispersion with a concentration of 1 mg / mL;

[0073] (11) Add 60 mg of ZnFe2O4@NC obtained in step (8) to the GO dispersion obtained in step (10), and after ultrasonic and mechanical stirring for 1 h each, add 180 μL of ethylenediamine and stir vigorously for 2 h;

[0074] (12) The above dispersion was transferred to a 100 mL reactor and subjected to hydrothermal reaction at 120 °C for 12 h;

[0075] (13) After the reaction, the mixture was naturally cooled to room temperature and washed with deionized water until the pH was neutral. The product was collected by magnetic separation, pre-frozen for 12 h, and then vacuum freeze-dried for 36 h to obtain NRGO / ZnFe2O4@NC nanocomposite material, which was labeled as S3.

[0076] The XRD spectrum of the product of Example 3 is as follows Figure 1 As shown. The positions at 2θ = 18.2°, 29.9°, 35.3°, 36.9°, 42.8°, 46.9°, 53.1°, 56.6° and 62.2° are consistent with the positions corresponding to the (111), (220), (311), (222), (400), (422), (511), (440) and (533) crystal planes of the ZnFe2O4 standard card (JCPDS Card No. 22-1012). The characteristic peak at 2θ = 24.7° corresponds to the (002) crystal plane of RGO. The Raman spectrum of the product of Example 3 is shown in Figure 2 S3 at 1588cm -1 (G band) and 1345cm -1 There are two obvious diffraction peaks near (D band), I D / I G The XPS spectrum of the product of Example 3 is shown in Figure 3 . Figure 3 (a) C, N, O, Fe and Zn elements were detected on the sample surface; Figure 3(b) is the spectrum of C1s, 284.8, 285.7 and 288.4 eV are the energy spectrum peaks of C=C / CC, CN and CO respectively; Figure 3 (c) is the N1s spectrum, 398.7, 400.0 and 401.7 eV are the characteristic peaks of pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen respectively; Figure 3 (d) is the O1s spectrum, 530.3, 531.8 and 533.4 eV are the energy spectrum peaks of metal-O, CO / C=O and CO respectively; Figure 3 (e) is the Fe 2p spectrum. The energy spectrum peaks at 726.0 and 712.4 eV are Fe 2p 1 / 2 and Fe2p 3 / 2 Characteristic peaks of Figure 3 (f) is the Zn 2p spectrum, 1021.7 and 1044.8 eV are Zn 2p 3 / 2 and Zn 2p 1 / 2 The SEM image of the product of Example 3 is shown in Figure 4 (g)-(i) show that the smooth surface of ZnFe2O4@NC microspheres is uniformly attached to the wrinkled NRGO surface. TEM images of the product of Example 3 are shown in Figure 4 (j) and (k) show that the ZnFe2O4@NC composite has ZnFe2O4 as the core and the NC layer of the shell is about 55nm. The product in Example 3 was mixed with paraffin wax, and a coaxial sample with an outer diameter of 7mm, an inner diameter of 3.04mm and a thickness of about 2mm was pressed in a special mold according to a filling ratio of 16.5wt.%. The electromagnetic parameters were tested with a Keysight E5080B vector network analyzer, and the wave absorption performance was calculated. The test frequency range is 2-18GHz. The reflection loss of sample S3 changes with frequency as shown in the following figure: Figure 7 As shown in Figure 1, when the matching thickness is 3.06 mm, the maximum absorption intensity reaches -61.1 dB at 11.3 GHz. When the matching thickness is 2.61 mm, the maximum effective absorption bandwidth is 7.2 GHz, covering the entire Ku band and part of the X band. By adjusting the thickness of the composite material, effective absorption of electromagnetic waves in different bands can be achieved. The eddy current coefficient of the product of Example 3 varies with frequency. Figure 8 In the range of 2-4 GHz, the eddy current coefficient decreases with frequency and reaches a maximum value, indicating that the magnetic loss is mainly due to natural resonance; it fluctuates in the range of 10-15 GHz, indicating that the magnetic loss is mainly due to exchange resonance; it remains basically unchanged in the range of 16-18 GHz, indicating that the magnetic loss is mainly due to eddy current loss. The attenuation constant of the product of Example 3 changes with frequency. Fig. 9 The larger the value, the stronger the attenuation capability. The attenuation constant of S3 increases gradually with the increase of frequency, and its maximum attenuation constant value is 161.1.

[0077] It can be seen from the test results of the above embodiments that the present invention adopts solvent thermal, self-polymerization, carbonization and hydrothermal steps to prepare nitrogen-doped reduced graphene oxide / zinc ferrite @ nitrogen-doped carbon nanocomposite absorbing materials. This method is green and safe, and no toxic substances are produced. The nanocomposite material has excellent absorbing properties, and achieves strong absorption (-61.1dB, 99.9999% absorption) and wide absorption bandwidth (7.2GHz, covering the entire Ku band and part of the X band) at a low filling ratio (16.5wt.%). By adjusting the composition and thickness of the composite material, effective absorption of electromagnetic waves in different bands can be achieved. Therefore, the prepared nitrogen-doped reduced graphene oxide / zinc ferrite @ nitrogen-doped carbon nanocomposite material has important application value in the field of electromagnetic wave absorption.

Claims

1. A nitrogen-doped reduced graphene oxide / zinc ferrite@nitrogen-doped carbon (NRGO / ZnFe 2 O 4 @NC) Preparation method of nanocomposite wave absorbing material, It is characterized in that The following steps are involved: (1) dissolving ferric chloride hexahydrate and zinc chloride in ethylene glycol solvent in sequence; (2) Sodium acetate and polyethylene glycol-6000 were added to the above solution, and the mixture was stirred in an oil bath at 55°C for 2 h to form a uniform mixture; (3) The above solution was transferred to a stainless steel reactor lined with polytetrafluoroethylene for solvothermal reaction; (4) After the reaction, the product was collected by magnetic separation, washed with anhydrous ethanol and deionized water until the pH was neutral, and freeze-dried at -50°C for 36 h; (5) ZnFe 2 O 4 Ultrasonic dispersion in tris(hydroxymethylaminomethane) buffer solution, then dopamine (DA) was added and stirred to carry out polymerization reaction; (6) the obtained product was washed with deionized water until the pH was neutral, and vacuum freeze-dried at -50°C for 36h to obtain zinc ferrite@polydopamine (ZnFe 2 O 4 @PDA); (7) the product was calcined at 500 °C for 2 h to obtain ZnFe 2 O 4 @NC; (8) ultrasonically dispersing multilayer graphene oxide (GO) in deionized water to form a uniform GO dispersion; (9) adding ZnFe 2 O 4 @NC and ethylenediamine (EDA); (10) the dispersion was transferred to a stainless steel reactor lined with polytetrafluoroethylene for hydrothermal reaction; (11) after the reaction, the product was washed with anhydrous ethanol and deionized water until the pH was neutral, and then freeze-dried at -50 °C for 36 h to obtain the target product NRGO / ZnFe 2 O 4 @NC nanocomposite absorbing material.

2. A NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: The iron salt in step (1) is ferric chloride hexahydrate, the zinc salt is zinc chloride, and the molar ratio of ferric chloride hexahydrate to zinc chloride is 2:

1.

3. A NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: In the step (2), the reagents need to be dissolved in sequence and then added separately.

4. The NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: The dissolution heat reaction temperature in step (3) is 200° C. and the time is 8 hours.

5. The NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: In the step (5), the solvent is 100 mL of deionized water, the amount of tris(hydroxymethyl)aminomethane added is 0.1212 g, the amount of DA added is 0.1 g, and the stirring time is 24 h.

6. The NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: In the step (8), the amount of graphite oxide added is 60 mg and the ultrasonic time is 30 min. The graphite oxide flakes are exfoliated and dispersed in deionized water to form a uniform GO dispersion.

7. The NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: In the step (9), ZnFe 2 O 4 @The amount of NC added was 60 mg, and the volume of EDA added was 180 μL.

8. The NRGO / ZnFe according to claim 1 2 O 4 @NC nanocomposite wave absorbing material preparation method, Features: The hydrothermal reaction temperature in step (10) is 120° C. and the reaction time is 12 h.

9. A nitrogen-doped reduced graphene oxide / zinc ferrite@nitrogen-doped carbon nanocomposite absorbing material, It is characterized in that Prepared by the method described in claims 1-8.

Citation Information

Patent Citations

  • Iron oxide-nitrogen doped carbon micro-tube composite wave-absorbing material and preparation method thereof

    CN110790316A

  • Nitrogen-doped graphene nickel ferrite composite wave-absorbing material and preparation method thereof

    CN112375541A

  • Nitrogen-doped graphene / cobalt-zinc ferrite composite aerogel wave-absorbing material and preparation method thereof

    CN112430451A

  • Nitrogen-sulfur doped porous carbon sphere modified ZnFe2O4 lithium ion battery negative electrode material and preparation method

    CN112607783A

  • Preparation method of nitrogen-doped porous carbon coated hollow cobalt-nickel alloy composite wave-absorbing material

    CN112743098A

Cited By

  • Lightweight heat-insulating multifunctional electromagnetic wave absorbing material with one-dimensional silicon carbide nanowires grown on two-dimensional reduced graphene oxide and preparation method of lightweight heat-insulating multifunctional electromagnetic wave absorbing material