Coal-based briquetted activated carbon-based carbon for protection and preparation method thereof

Through the ratio of weakly caking coal and long-flame coal and the pre- and post-oxidation treatment, the pore structure of activated carbon is optimized, which solves the problems of low strength and short protection time of columnar carbon for protection, and achieves higher protection performance and longer service life. time.

CN118851175APending Publication Date: 2024-10-29SHENHUA XINJIANG ENERGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410873380.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing columnar carbon for protection has low strength and short protection time, which results in the generation of dust during protective use, which is detrimental to the human respiratory system and limits the protection time, making it difficult to extend it.

Method used

The ratio of weakly caking coal and long-flame coal is used for grinding and briquetting. It combines pre-oxidation, carbonization, post-oxidation and activation treatments to optimize the pore structure and improve the strength and protective performance of activated carbon.

Benefits of technology

The strength and protection time of coal-based briquette activated carbon for protection are significantly improved, dust generation is reduced, the protection time is extended, and the protective performance of activated carbon is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004922264010000041
    Figure BDA0004922264010000041
  • Figure BDA0004922264010000051
    Figure BDA0004922264010000051
  • Figure BDA0004922264010000052
    Figure BDA0004922264010000052
Patent Text Reader

Abstract

The invention discloses coal-based briquetting activated carbon-based carbon for protection and a preparation method thereof. The preparation method comprises the following steps: step a, selecting weakly caking coal and long flame coal as raw materials, and grinding to obtain raw material coal; step b, briquetting the raw material coal, forming, and granulating to obtain a briquetting material; c, carrying out pre-oxidation treatment, carbonization and post-oxidation treatment on the briquetting material to obtain a carbonized material; and step d, performing activation improvement treatment on the carbonized material to prepare the coal-based briquetting activated carbon-based carbon for protection. According to the technical scheme provided by the invention, the weakly caking coal and the long flame coal are matched, so that the strength of the briquetting activated carbon is enhanced; by adding pre-oxidation and post-oxidation treatment for a certain time before and after the carbonization process, the pore structure is optimized, the protection time is prolonged, the strength is increased, and the protection performance of the briquette activated carbon is optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of protection, and in particular to a coal-based compressed activated carbon-based carbon for protection and a preparation method thereof. Background Art

[0002] Protective coal-based activated carbon is an activated carbon product used in the field of gas phase adsorption, and usually plays a role in individual and collective protection devices. At present, protective coal-based activated carbon at home and abroad is mainly columnar carbon, and its particle size is generally 0.9mm or 1.5m. On the one hand, this type of activated carbon is directly used as a base carbon for physical adsorption; on the other hand, it can be treated through an impregnation process to form impregnated activated carbon for physical-chemical combined protection. Due to the limitations of the preparation process of columnar carbon and the properties of the finished product, its strength is generally between 85% and 90%, which will affect its service life; in addition, the protective performance of columnar carbon, that is, the protection time, has certain limitations and is difficult to extend, and its application is subject to certain restrictions.

[0003] At present, most of the columnar carbon used for protection is made of anthracite as raw material, and is prepared by processes such as grinding, pressing, carbonization and activation. The main defects are: (1) low strength, usually between 85% and 90%, which leads to the generation of more dust during the protective use, causing adverse effects on the human respiratory system; (2) the protection time parameters need to be extended. The benzene protection time is about 45 minutes, and the ethyl chloride protection time is about 27 minutes, which limits the escape time of the protective personnel during use and also brings certain difficulties to the actual protection process. Summary of the invention

[0004] The present invention aims to provide a protective coal-based briquette activated carbon-based carbon and a preparation method thereof, so as to improve the strength of the protective coal-based activated carbon.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing protective coal-based compressed activated carbon is provided. The preparation method comprises the following steps: step a, selecting weakly sticky coal and long flame coal as raw materials, grinding to obtain raw coal; step b, briquetting and granulating the raw coal to obtain compressed materials; step c, performing pre-oxidation treatment, carbonization and post-oxidation treatment on the compressed materials to obtain carbonized materials; step d, performing activation and improvement treatment on the carbonized materials to obtain protective coal-based compressed activated carbon.

[0006] Furthermore, the mass ratio of the weakly sticky coal to the long flame coal is 6-8:2-4.

[0007] Furthermore, in step a, after grinding, the content of raw coal powder with a particle size less than 44 μm is not less than 70%, and preferably the content of coal powder with a particle size less than 44 μm is 75% to 80%.

[0008] Furthermore, in step b, the pressure during the briquetting of the raw coal is 20Mpa-30Mpa.

[0009] Furthermore, in step b, granulation includes crushing and screening to obtain coal particles with a particle size of 1 mm to 10 mm, more preferably 3 mm to 8 mm.

[0010] Furthermore, in step c, the pre-oxidation treatment conditions are: the compressed material is oxidized at 200-255° C., preferably 240-250° C., for 3-5 hours, and the oxygen content in the oxidizing atmosphere is 6-12 vol%.

[0011] Furthermore, the oxidizing atmosphere is formed by using a mixture of nitrogen and air as an oxidant.

[0012] Furthermore, the conditions for carbonization and post-oxidation treatment are: temperature 500-555°C, oxygen content of carbonization atmosphere not more than 3 vol%, and carbonization treatment time 2-3 hours; preferably, the compressed material is heated from 250°C to 550-555°C at a heating rate of 8-10°C / min, and after the carbonization reaction is completed, the temperature is reduced to 250°C 240-250°C, kept warm for 0.5-1 hour, and then subjected to step-by-step cooling treatment; preferably, the cooling rate of the step-by-step cooling treatment is 30-50°C / h.

[0013] Furthermore, in step d, the conditions for the activation treatment are: using water vapor as an activating agent, carrying out an activation reaction at 900-920°C, and the reaction time is 4.5 to 5.5 hours; preferably, after the carbonized material is heated to 880-900°C at a heating rate of no more than 20°C / min, water vapor is introduced to carry out the activation reaction, and the temperature is continued to be raised to 900-920°C for stable activation for 4.5 to 5.5 hours.

[0014] According to another aspect of the present invention, there is provided a protective coal-based compressed activated carbon-based carbon, which is prepared according to the preparation method of protective coal-based compressed activated carbon-based carbon according to any one of claims 1 to 9.

[0015] By applying the technical solution of the present invention, the strength of the briquette activated carbon is enhanced by mixing weakly sticky coal and long flame coal; by adding a certain period of pre-oxidation and post-oxidation treatment before and after the carbonization process, the pore structure is optimized, the protection time is extended and the strength is increased, and the protection performance of the briquette activated carbon is optimized. DETAILED DESCRIPTION

[0016] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0017] Glossary:

[0018] Protective carbon: It is a general term for activated carbon mainly used in the fields of individual protective equipment and collective protective equipment.

[0019] Base carbon: refers to activated carbon with good impregnation basic properties, which can achieve physical-chemical combined adsorption synergy through processes such as impregnation with different chemical reagents.

[0020] Oxidation reaction: It is a process in which the raw coal is subjected to low-temperature carbonization reaction under the condition of contact with air, thereby effectively reducing non-carbon elements, generating an oxide material with a preliminary developed pore structure, and ensuring that it has high mechanical strength.

[0021] Coal blending technology: also known as coal blending method, is a technology that analyzes the grindability, calorific value, ash composition and ash melting point of different raw coals, and combines different types of coal in proportion according to the requirements of preparing the target activated carbon strength, pore structure and adsorption performance, so as to produce high-quality activated carbon products.

[0022] Weakly sticky coal: Bituminous coal with a low degree of coalification and a wide range of volatiles. Few colloids are generated after heating, with only weak cohesiveness. There are more silky and semi-silky groups in the microscopic components of the coal rock.

[0023] Long flame coal: A type of bituminous coal with the lowest degree of metamorphism, ranging from non-caking to weakly caking. The youngest of them also contain a certain amount of humic acid. It is easy to weather and break when stored. Old coal with a high degree of coalification can produce a certain amount of colloid when heated.

[0024] In view of a series of technical problems described in the background technology, according to a typical implementation of the present application, a method for preparing coal-based compressed activated carbon-based carbon for protection is provided to solve the problems of low strength and unsatisfactory protection time performance of columnar carbon in applications in the protection field.

[0025] At the same time, most of the products used in the protection field are columnar carbon products, and there is no precedent for the application of compressed activated carbon. Therefore, the technical solution of this application can, on the one hand, enhance the strength and protective performance of activated carbon for protection, and on the other hand, fill the application gap of compressed activated carbon in the protection field.

[0026] According to a typical embodiment of the present application, a method for preparing a protective coal-based compressed activated carbon-based carbon is provided. The preparation method comprises the following steps: step a, selecting weakly sticky coal and long flame coal as raw materials, grinding to obtain raw coal; step b, briquetting and granulating the raw coal to obtain compressed materials; step c, performing pre-oxidation treatment, carbonization and post-oxidation treatment on the compressed materials to obtain carbonized materials; step d, performing activation and improvement treatment on the carbonized materials to obtain protective coal-based compressed activated carbon-based carbon.

[0027] By applying the technical solution of the present invention, the strength of the briquette activated carbon is enhanced by mixing weakly sticky coal and long flame coal; by adding a certain period of pre-oxidation and post-oxidation treatment before and after the carbonization process, the pore structure is optimized, the protection time is extended and the strength is increased, and the protection performance of the briquette activated carbon is optimized.

[0028] Preferably, the mass ratio of weakly sticky coal to long flame coal is 10-8:0-2..., preferably 8:2. Within this ratio range, the strength of the briquette activated carbon is greatly improved.

[0029] In one embodiment of the present application, in step a, weakly sticky coal and long flame coal are selected as raw materials, and after optimizing the ratio, raw coal is ground to obtain raw coal. The specific coal grinding process is well known in the art, and the raw coal is ground to a finer powder, for example, through a 180 mesh, 200 mesh, and 325 mesh Taylor standard sieve. In a preferred embodiment of the present invention, the raw coal is ground to obtain coal powder with a specific particle size distribution, wherein in step a, after grinding, the raw coal powder with a particle size of less than 44 μm accounts for no less than 70%, and preferably the mass proportion of coal powder with a particle size of less than 44 μm is 75% to 80%. Within this proportion range, the strength of the briquette activated carbon is optimal. Of course, other content ratios within the scope of the present application may also be possible, for example, the content of coal powder with a particle size less than 44 μm is 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 99%, 99% or 100%.

[0030] In the present application, step b is to briquette and granulate the above raw coal to obtain coal particles. In the preparation of coal-based briquette activated carbon, the molding and crushing and granulation of coal powder is a conventional process in the field, such as using a roller briquetting machine to mold coal powder, such as using a crusher to crush, and then screening to obtain coal particles with a certain particle size range. According to a typical embodiment of the present application, the briquetting pressure of the raw coal is 20Mpa~30Mpa; granulation includes crushing and screening to obtain coal particles with a particle size of 1mm~10mm, more preferably 3mm~8mm. By controlling these technical parameters, the strength and other indicators of the obtained base carbon are further optimized.

[0031] In the present application, step c is to perform pre-oxidation treatment, carbonization treatment, and post-oxidation treatment on the coal particles to obtain a carbonized material. According to a specific embodiment, the pre-oxidation treatment conditions are: at 200-255°C, for example, 240-250°C, the material is oxidized for 3-5 hours, preferably 3 hours, and the oxygen content in the oxidizing atmosphere is 6-12 vol%, for example, a mixture of nitrogen and air is used as an oxidant to form an oxidizing atmosphere, so that the oxidation of the material is controlled to a lighter degree, so that part of the oxygen is combined with the coal, and the activation reaction rate is accelerated.

[0032] According to a typical implementation of the present application, the carbonization and post-oxidation treatment conditions are: temperature 500-555°C, carbonization atmosphere oxygen content not more than 3 vol%, carbonization treatment time 2-3 hours, preferably 2.5 hours, preferably, the material is heated from 250°C to 550°C at a heating rate of 8-10°C / min. After the carbonization reaction is completed, when the temperature drops to about 240-250°C, the material is kept at this temperature for 0.5-1 hour, and then a step-by-step cooling treatment is performed, and the cooling rate of the step-by-step cooling treatment is 50°C / h.

[0033] According to a typical implementation of the present application, the activation treatment conditions in step d are: using water vapor as an activator, carrying out an activation reaction at 900-920°C, and the reaction time is 4.5 hours to 5.5 hours. Preferably, after the carbonized material is heated to 880-900°C at a heating rate of not more than 20°C / min, water vapor is introduced to carry out the activation reaction, and the temperature is continued to be raised to 900-920°C for stable activation for 4.5 to 5.5 hours.

[0034] In terms of preparation process, the present application optimizes the pore structure, prolongs the protection time and increases the strength, thereby optimizing the protection performance of the compressed activated carbon by adding a certain period of pre-oxidation and post-oxidation treatment before and after the carbonization process and reducing process parameters such as activation time, temperature and amount of activator added.

[0035] According to a typical embodiment of the present application, a protective coal-based compressed activated carbon-based carbon is provided. The protective coal-based compressed activated carbon-based carbon is prepared according to any of the above-mentioned preparation methods of protective coal-based compressed activated carbon-based carbon.

[0036] The beneficial effects of the present invention will be further described below in conjunction with embodiments.

[0037] Example 1

[0038] 1. Preparation of protective briquetted activated carbon from single coal

[0039] 100% A coal (weakly sticky coal) and G coal (long flame coal) briquette samples were prepared. The specific method was as follows: a certain amount of A or G coal was dried to a moisture content of 3%-4%, and then ground using a coal mill. The raw coal powder with a particle size of less than 44 μm after grinding contained 72% of the raw coal powder. Then, a briquetting machine was used for molding and granulation to obtain briquette materials. The briquette materials were added to a carbonization furnace for pre-oxidation for 3 hours, carbonization for 2.5 hours, and post-oxidation for 0.5 hours to obtain carbonized materials. The final carbonization temperature was set to 550°C. The carbonized materials were added to an activation furnace for activation treatment. The activation end temperature was set to 900°C. The activation time was 240 minutes. The activator used water vapor, and the water-carbon ratio was 2:1. The experimental results are shown in Table 1. In the experiment, sample 1# was a sample prepared with 100% A coal as raw material, and sample 2# was a sample prepared with 100% G coal as raw material. It can be seen from the experimental results that both A coal and G coal can be used alone as raw coal to produce activated carbon. In general, the yield of activated carbon samples prepared from coal A is slightly lower than that from coal G, which is due to its lower degree of metamorphism and higher volatile matter.

[0040] Table 1 Process conditions and test results of activated carbon produced from single coal

[0041]

[0042]

[0043] 2. Preparation of protective briquetted activated carbon by coal blending method

[0044] In this experiment, A coal and G coal were used to prepare briquette activated carbon. A certain amount of A and G coal were dried to a moisture content of 3%-4%, and then quantitatively added to the coal mill for grinding. The raw coal powder with a particle size of less than 44μm after grinding contained 72%. Then, a briquette machine was used for molding and granulation to obtain briquette material. The briquette material was added to a carbonization furnace for pre-oxidation for 3h, carbonization for 2.5h, and post-oxidation for 0.5h to obtain carbonized material. The final carbonization temperature was set to 550℃. The carbonized material was added to an activation furnace for activation treatment. The activation end temperature was set to 900℃, and the activation time was 240min. Water vapor was used as the activator, and the water-carbon ratio was 2:1. A total of 2 groups of coal blending experiments were conducted. The mass ratios of A coal and G coal were 8:2 and 5:5, respectively, and were marked as 3# and 4#, respectively. The experimental results are shown in Table 2. From the results, it can be seen that under the same carbon activation conditions, the addition of a small amount of G coal has a certain impact on the various indicators of activated carbon, but with the increase of G coal addition, the wear resistance is improved, the packing density is slightly increased, and the other indicators do not change much.

[0045] Table 2 Test results of coal blending for preparing protective briquetted activated carbon

[0046]

[0047]

[0048] It can be seen from the above table that the performance test results of sample 3# are better than those of samples with other numbers. Therefore, the ratio of raw coal is determined to be A:G=8:2, and subsequent experiments are carried out based on this ratio.

[0049] 3. Preparation of protective briquetted activated carbon by pre-oxidation, carbonization and post-oxidation

[0050] In this experiment, the ratio of A coal: G coal is 8:2. In the pre-oxidation, carbonization and post-oxidation processes, the specific method is: the briquette material is added to the carbonization furnace at room temperature. The pre-oxidation process is to pass a mixture of nitrogen and air into the furnace as an oxidant to form an oxidizing atmosphere. The oxygen content in the oxidizing atmosphere is 6 vol%. It is oxidized at 250 ° C. The carbonization process starts from 250 ° C and is heated to 550 ° C at a heating rate of 10 ° C / min. After the carbonization reaction is completed, the temperature is reduced to 250 ° C, kept warm for 0.5 hours, and then a step-by-step cooling treatment is performed to prepare briquette activated carbon. A total of two groups of experiments were carried out, and the experimental conditions were 5#: no oxidation process; 6# with oxidation process. The experimental results are shown in Table 3. It can be seen from the results that under the same ratio conditions, adding pre-oxidation and post-oxidation processes can improve the strength of briquette activated carbon and extend the protection time to a certain extent.

[0051] Table 3 Test results of protective briquetted activated carbon prepared with and without oxidation process

[0052]

[0053]

[0054] 4. Preparation of protective activated carbon briquettes under different activation conditions

[0055] A sample with a ratio of A coal to G coal of 8:2 was selected. After pre- and post-oxidation process treatment, the activation time, activation temperature and water-to-carbon ratio were adjusted to carry out experiments, as shown in Table 4.

[0056] Table 4 Activation process adjustment to prepare protective briquetted activated carbon test results

[0057]

[0058] (1) Influence of activation time

[0059] 7# and 8# are two groups of experiments with different activation time conditions. It was found that with the increase of activation time, the activation yield changed slightly, and the decrease of activation yield resulted in no obvious growth trend of indicators such as iodine adsorption value.

[0060] From the perspective of industrial production, although extending the activation time can slightly increase the adsorption capacity and protection time of activated carbon, the decrease in output and yield makes it not suitable as a means to improve the adsorption capacity of the product.

[0061] (2) Effect of activation temperature

[0062] In order to improve the activation depth, the effect of increasing the activation temperature on the production of compressed activated carbon was further investigated. Experiments were conducted at activation temperatures of 920°C and 950°C, and the results were marked as 9# and 10#, as shown in Table 4. By increasing the temperature, the activation yield decreased significantly, and the iodine adsorption value increased significantly, reaching 1224 mg / g at 950°C. Although increasing the temperature and deepening the degree of activation make the pore structure of the activated carbon richer and the protection time slightly increased, the wear resistance is not much different, and the ash content is slightly increased due to the decrease in yield.

[0063] (3) Impact of water-carbon ratio

[0064] Increasing the water-carbon ratio is also a common means of adjusting the activation depth. In the experiment, we further increased the water-carbon ratio to 2.5:1 and 3:1, and the sample results were recorded as 11# and 12# to examine the effect of different water-carbon ratios on the activation process. Increasing the water-carbon ratio has little effect on the adsorption performance and protection time of the product, indicating that under the condition of excess water vapor, further increasing the amount of water vapor has limited effect on improving the adsorption value and protection time.

[0065] Finally, the optimal preparation method was determined as follows: coal blending → pulverizing → briquetting → pre-oxidation → carbonization → post-oxidation → activation → performance testing → briquetting protective activated carbon

[0066] Among them, coal blending A:G=8:2; pulverizing: coal powder fineness 325 mesh 90% passed; briquetting: according to high-strength briquetting conditions; pre-oxidation: oxidation at 240-260℃ for 3h; carbonization at 580-600℃ for 2.5h; post-oxidation: oxidation at 240-260℃ for 1h; activation temperature 920℃, activator carbon ratio 2.5:1, activation time 270 minutes.

[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a protective coal-based activated carbon briquette, characterized in that: The steps include: Step a, selecting weakly sticky coal and long flame coal as raw materials, grinding to obtain raw coal; Step b, briquetting and granulating the raw coal to obtain briquette material; Step c, performing pre-oxidation treatment, carbonization and post-oxidation treatment on the briquette material to obtain a carbonized material; Step d, performing activation and improvement treatment on the carbonized material to obtain the protective coal-based compressed activated carbon-based carbon.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the weakly sticky coal to the long flame coal is 6-8:2-4.

3. The preparation method according to claim 1, characterized in that: In the step a, after the grinding, the content of raw coal powder with a particle size less than 44 μm is not less than 70%, and preferably the content of coal powder with a particle size less than 44 μm is 75% to 80%.

4. The preparation method according to claim 1, characterized in that: In the step b, the pressure during the molding of the raw coal briquette is 20Mpa-30Mpa.

5. The preparation method according to claim 1, characterized in that: In the step b, the granulation includes crushing and screening to obtain coal particles with a particle size of 1 mm to 10 mm, more preferably 3 mm to 8 mm.

6. The preparation method according to claim 1, characterized in that: In the step c, the pre-oxidation treatment conditions are: oxidation treatment of the pressed material at 200-255° C., preferably 240-250° C., for 3-5 hours, and the oxygen content in the oxidizing atmosphere is 6-12 vol%.

7. The preparation method according to claim 6, characterized in that: The oxidizing atmosphere is formed by using a mixture of nitrogen and air as an oxidant.

8. The preparation method according to claim 1, characterized in that: The conditions of the carbonization and post-oxidation treatment are: temperature 500-555°C, oxygen content of the carbonization atmosphere not more than 3 vol%, and carbonization treatment time 2-3 hours; Preferably, the briquetting material is heated from 250°C to 550-555°C at a heating rate of 8-10°C / min, and after the carbonization reaction is completed, the temperature is reduced to 240-250°C, kept at this temperature for 0.5-1 hour, and then subjected to a step-by-step cooling treatment; Preferably, the cooling rate of the step-by-step cooling treatment is 30-50°C / h.

9. The preparation method according to claim 1, characterized in that: In step d, the activation treatment conditions are: using water vapor as an activating agent, performing the activation reaction at 900-920° C., and the reaction time is 4.5 to 5.5 hours; Preferably, after the carbonized material is heated to 880-900°C at a heating rate of no more than 20°C / min, water vapor is introduced to perform an activation reaction, and the temperature is continued to be raised to 900-920°C for stable activation for 4.5 to 5.5 hours.

10. A protective coal-based briquette activated carbon-based carbon, characterized in that: It is prepared according to the method for preparing protective coal-based compressed activated carbon-based carbon as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Active brown coal and preparation method thereof

    CN102583322A

  • Micro-granularity coal-based activated carbon and preparation method thereof

    CN107416825A

  • Method for preparing active carbon with developed mesopores by using coal

    CN108439399A

  • Preparation method of activated carbon for solvent recovery

    CN109824049A

  • Activated carbon prepared from waste carbonized material powder as well as preparation method and application thereof

    CN111573668A