Method for solid-phase synthesis of molecular sieve by taking rice husk as silicon source and template

The preparation of molecular sieves through solid-phase synthesis of rice husk solves the problems of wastewater discharge and high cost in traditional methods, achieves the preparation of high crystallinity and environmentally friendly molecular sieves, and promotes the high value-added utilization of agricultural waste.

CN118851202AActive Publication Date: 2024-10-29HUAQIAO UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410911552.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The traditional hydrothermal method produces a large amount of wastewater during the preparation of molecular sieves, resulting in environmental pollution and high production costs.

Method used

Rice husk is used as the silicon source and template, and through the steps of room temperature immersion, oil bath heating, crystallization and high-temperature roasting, combined with structure-directing agents such as tetrapropylammonium hydroxide and n-butylamine, solid-phase synthesis of molecular sieves is performed to precisely control crystallization. Temperature and time to remove organic cellulose and template components.

Benefits of technology

It achieves the preparation of molecular sieves with high crystallinity, reduces wastewater discharge, is simple and energy-saving, promotes the high value-added utilization of agricultural waste, and achieves environmentally friendly resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851202A_ABST
    Figure CN118851202A_ABST
Patent Text Reader

Abstract

The invention discloses a method for solid-phase synthesis of a molecular sieve by taking rice hulls as a silicon source and a template, which comprises the following steps: (1) soaking rice hull powder in a hydrochloric acid solution, heating in an oil bath to remove impurities in the rice hull powder, washing the obtained suspension with deionized water to be neutral, and drying in a drying oven; (2) fully grinding and uniformly mixing the material obtained in the step (1), a structure-directing agent, NaAlO2 and NaOH, and then crystallizing, the structure-directing agent being tetrapropylammonium hydroxide and / or n-butylamine; and (3) roasting the material obtained in the step (2) at high temperature to remove the organic cellulose and the template component, thereby obtaining the molecular sieve. The method effectively solves the problems of large wastewater discharge amount and high cost in the traditional molecular sieve preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste biomass resource utilization, and specifically relates to a method for solid-phase synthesis of molecular sieves using rice husks as a silicon source and template. Background Art

[0002] According to the grain production data released by the National Bureau of Statistics, my country's total rice production reached 206.6 million tons in 2023. As one of the main agricultural by-products of processed rice, rice husk accounts for about 20% of the total mass of rice, which is about 41.32 million tons. Traditionally, rice husks, as agricultural waste, are often directly burned or abandoned, which has a serious impact on the environment. However, with people's increasing attention to sustainable development and resource recycling, the rational resource utilization of rice husks has been given new value. Studies have shown that the silicon content of rice husk products that have been fully roasted at high temperature can reach more than 90%, which makes silicon-rich rice husks have potential application value in the preparation of molecular sieve materials.

[0003] Molecular sieves have been widely used in catalytic thermal cracking reactions due to their excellent thermal stability, suitable acid properties and unique pore structure. However, the traditional hydrothermal method for preparing molecular sieves produces a large amount of wastewater, which not only pollutes the environment but also increases production costs. Therefore, it is of great significance to develop a simple and environmentally friendly molecular sieve preparation technology.

[0004] CN 105731485A discloses a method for preparing a multi-level pore zeolite molecular sieve using rice husks. The synthesis process consumes a large amount of water, and the specific synthesis steps are as follows: 30-35 parts of rice husks, 5-8 parts of NaAlO2, 45-55 parts of deionized water, 3-5 parts of NaOH and 0.5-0.8 parts of TPAOH are selected by weight, mixed and stirred evenly, and added to a stainless steel reactor, heated to 150-160°C, reacted for 20-30 hours, taken out, centrifuged to obtain a precipitate, rinsed with deionized water 2-4 times, and then dried in an oven at 80-100°C. After drying, the precipitate is placed in a muffle furnace, roasted at 500-600°C for 4-6 hours, and the resulting crystals are taken out after cooling. Next, 5-7g NaAlO2 and 20-25g NaOH are dissolved in 600-650mL distilled water, stirred until the solid is completely dissolved, and then 50-60g white carbon black is added, and the mixture is stirred and mixed for 2-3h to form a gel. 3-5% of the above crystals are added to the gel as seeds, and after being stirred and dispersed evenly, the mixed gel is added to a stainless steel reactor and crystallized at 130-140°C for 50-80h. After the crystallization is completed, the product is repeatedly rinsed with deionized water until the filtrate is neutral, and then the rinsed product is placed in an oven at 100-120°C and dried for 6-8h to obtain a multi-stage pore zeolite molecular sieve. Although the above-mentioned prior art successfully prepares molecular sieves using rice husks, its preparation process is complicated and produces a large amount of wastewater. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for solid phase synthesis of molecular sieves using rice husks as a silicon source and template.

[0006] The technical solution of the present invention is as follows:

[0007] A method for solid phase synthesis of molecular sieves using rice husks as a silicon source and template comprises the following steps:

[0008] (1) soaking the rice husk powder in a hydrochloric acid solution at room temperature for 6-24 hours, then heating it in an oil bath at 80-130° C. for 10 minutes to 1 hour to remove impurities therein, then washing the obtained suspension with deionized water until it is neutral, and then drying it in an oven;

[0009] (2) the material obtained in step (1), a structure directing agent, NaAlO2 and NaOH are fully ground and mixed in a ratio of 1.8-2.2 g: 3.5-4.5 mL: 0.008-0.012 g: 0-0.12 g, and then crystallized at 100-200° C. for 10-48 h, wherein the structure directing agent is tetrapropylammonium hydroxide and / or n-butylamine;

[0010] (3) The material obtained in step (2) is subjected to high temperature roasting at 500-600° C. for 1-3 hours to remove organic cellulose and template components, thereby obtaining the molecular sieve.

[0011] In a preferred embodiment of the present invention, in step (1), the concentration of the hydrochloric acid solution is 2-15 wt%.

[0012] Further preferably, in the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g:1-2 L.

[0013] In a preferred embodiment of the present invention, in the step (2), the crystallization temperature is 110-170° C. and the time is 12-48 hours.

[0014] In a preferred embodiment of the present invention, in the step (3), the high temperature calcination is carried out at a temperature of 540-560°C and a time of 1.5-2.5 hours.

[0015] Further preferably, in the step (3), the heating rate of the high temperature calcination is 2-5°C / min.

[0016] In a preferred embodiment of the present invention, in step (1), the concentration of the hydrochloric acid solution is 2-15wt%; in step (2), the crystallization temperature is 110-170°C and the time is 12-48h; in step (3), the high temperature calcination temperature is 540-560°C and the time is 1.5-2.5h.

[0017] Further preferably, in the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g:1-2 L.

[0018] Further preferably, in the step (3), the heating rate of the high temperature calcination is 2-5°C / min.

[0019] Further preferably, in the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g:1-2 L; and in the step (3), the heating rate of the high temperature calcination is 2-5° C. / min.

[0020] The beneficial effects of the present invention are:

[0021] 1. The present invention uses rice husk as a silicon source and template agent to prepare molecular sieves by a simple solid phase synthesis method. During the synthesis process, by accurately controlling key parameters such as crystallization temperature, crystallization time, type of template agent and its dosage, a molecular sieve with high crystallinity can be prepared. This method effectively solves the problems of large wastewater discharge and high cost in the preparation process of traditional molecular sieves.

[0022] 2. The method of the present invention is simple, energy-saving and environmentally friendly, and can also promote the high-value-added utilization of agricultural waste, achieving the dual benefits of waste resource utilization and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The X-ray diffractometer spectra of the molecular sieves obtained under different synthesis conditions in Examples 1 to 8 of the present invention are shown in Figure 1. The crystal form is characterized by an X-ray powder diffractometer produced by Rigaku, model SmartLab, which is equipped with a Cu Kα radiation source of 40 kV and 30 mA. The detection range is 5-50°.

[0024] Figure 2 These are scanning electron microscope photographs of the molecular sieves prepared in Examples 1 to 8 of the present invention. The morphology was characterized using a field emission scanning electron microscope produced by Hitachi, with the equipment model being SU5500. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0026] Example 1

[0027] (1) 70 g of rice husk powder (mesh size 120) was soaked in 1 L of 5 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 100 °C for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80 °C for 12 h;

[0028] (2) 2 g of the material obtained in step (1), 4 mL of structure directing agent TPAOH, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high pressure reactor at 110° C. for 30 h;

[0029] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining Figure 1 The molecular sieve shown.

[0030] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The diffraction peaks of the sample are consistent with the diffraction peaks of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 1 is 90.2%. Figure 2 As shown in (a), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0031] Example 2

[0032] (1) 70 g of rice husk powder (mesh size 120) was soaked in 1 L of 5 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 100 °C for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80 °C for 12 h;

[0033] (2) 2 g of the material obtained in step (1), 4 mL of structure directing agent TPAOH, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high pressure reactor at 140° C. for 12 h;

[0034] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining Figure 1 The molecular sieve shown.

[0035] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 2 is 91.8%. Figure 2 As shown in (b), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0036] Example 3

[0037] (1) 70 g of rice husk powder (mesh size 120) was soaked in 1 L of 5 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 100 °C for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80 °C for 12 h;

[0038] (2) 2 g of the material obtained in step (1), 4 mL of structure directing agent TPAOH, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high pressure reactor at 140° C. for 48 h;

[0039] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining Figure 1 and Figure 2 The molecular sieve shown.

[0040] Figure 1The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 3 is 92.5%. Figure 2 As shown in (c), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0041] Example 4

[0042] (1) 70 g of rice husk powder (mesh size 120) was soaked in 1 L of 5 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 100 °C for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80 °C for 12 h;

[0043] (2) 2 g of the material obtained in step (1), 4 mL of structure directing agent TPAOH, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high pressure reactor at 170° C. for 30 h;

[0044] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining Figure 1 and Figure 2 The molecular sieve shown.

[0045] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 4 is 93.3%. Figure 2 As shown in (d), the molecular sieve prepared in this example mainly presents a block-like microstructure after being magnified by a scanning electron microscope.

[0046] Example 5

[0047] (1) 50 g of rice husk powder (mesh size 120) was soaked in 2 L of 2 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 130 ° C for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80 ° C for 12 h;

[0048] (2) 2 g of the material obtained in step (1), 2 mL of structure directing agent TPAOH, 2 mL of structure directing agent n-butylamine, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high pressure reactor at 170° C. for 30 h;

[0049] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 5° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining the molecular sieve.

[0050] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The diffraction peaks of the sample are consistent with the diffraction peaks of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 5 is 93.5%. Figure 2 As shown in (e), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0051] Example 6

[0052] (1) 80 g of rice husk powder (mesh size 120) was soaked in 1 L of 10 wt% hydrochloric acid solution at room temperature for 12 h, and then heated in an oil bath at 80° C. for 60 min to remove impurities therein, and then the obtained suspension was washed with deionized water until neutral, and then dried in an oven at 80° C. for 12 h;

[0053] (2) 2 g of the material obtained in step (1), 1 mL of structure-directing agent TPAOH, 3 mL of structure-directing agent n-butylamine, and 0.01 g of NaAlO2 were thoroughly ground and mixed, and then crystallized in a high-pressure reactor at 170° C. for 30 h;

[0054] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining the molecular sieve.

[0055] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 6 is 94.3%. Figure 2 As shown in (f), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0056] Example 7

[0057] (1) 80 g of rice husk powder (mesh size 120) was soaked in 1 L of 15 wt% hydrochloric acid solution at room temperature for 12 h, and then heated in an 80°C oil bath for 10 min to remove impurities therein, and then the obtained suspension was washed with deionized water until neutral, and then dried in an 80°C oven for 12 h;

[0058] (2) 2 g of the material obtained in step (1), 3 mL of structure-directing agent TPAOH, 1 mL of structure-directing agent n-butylamine, and 0.01 g of NaAlO2 were fully ground and mixed, and then crystallized in a high-pressure reactor at 170° C. for 30 h;

[0059] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 2° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining the molecular sieve.

[0060] Figure 1 The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 7 is 95.2%. Figure 2 As shown in (g), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0061] Example 8

[0062] (1) 50 g of rice husk powder (mesh size 120) was soaked in 1 L of 2 wt% hydrochloric acid solution at room temperature for 24 h, and then heated in an oil bath at 130° C. for 30 min to remove impurities therein. The resulting suspension was then washed with deionized water until neutral, and then dried in an oven at 80° C. for 12 h;

[0063] (2) 2 g of the material obtained in step (1), 4 mL of structure directing agent TPAOH, 0.01 g of NaAlO2, and 0.12 g of NaOH (used to control the morphology and particle size of the molecular sieve) were fully ground and mixed, and then crystallized at 170° C. for 30 h in a high-pressure reactor;

[0064] (3) placing the material obtained in step (2) in a muffle furnace, heating it to 550° C. at a rate of 5° C. / min, and then calcining it at 550° C. for 2 h to remove the organic cellulose and template components, thereby obtaining the molecular sieve.

[0065] Figure 1The XRD spectrum results show that the molecular sieve prepared in this example has good crystallinity. The sample diffraction peak is consistent with the diffraction peak of the standard card (JCPDS No.44-0003). The crystallinity of the sample is calculated within the diffraction angle range of 15-30°. The crystallinity of Example 8 is 94.7%. Figure 2 As shown in (h), the molecular sieve prepared in this example has a block-like microstructure after being magnified by a scanning electron microscope.

[0066] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for solid phase synthesis of molecular sieves using rice husks as silicon source and template, characterized in that: The steps include: (1) soaking the rice husk powder in a hydrochloric acid solution at room temperature for 6-24 hours, then heating it in an oil bath at 80-130° C. for 10 minutes to 1 hour to remove impurities therein, then washing the obtained suspension with deionized water until it is neutral, and then drying it in an oven; (2) the material obtained in step (1), a structure directing agent, NaAlO2 and NaOH are fully ground and mixed in a ratio of 1.8-2.2 g: 3.5-4.5 mL: 0.008-0.012 g: 0-0.12 g, and then crystallized at 100-200° C. for 10-48 h, wherein the structure directing agent is tetrapropylammonium hydroxide and / or n-butylamine; (3) The material obtained in step (2) is subjected to high temperature roasting at 500-600° C. for 1-3 hours to remove organic cellulose and template components, thereby obtaining the molecular sieve.

2. The method according to claim 1, characterized in that: In the step (1), the concentration of the hydrochloric acid solution is 2-15 wt %.

3. The method according to claim 2, characterized in that: In the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g: 1-2 L.

4. The method according to claim 1, characterized in that: In the step (2), the crystallization temperature is 110-170° C. and the crystallization time is 12-48 hours.

5. The method according to claim 1, characterized in that: In the step (3), the high temperature calcination temperature is 540-560°C and the time is 1.5-2.5h.

6. The method according to claim 5, characterized in that: In the step (3), the heating rate of the high temperature calcination is 2-5°C / min.

7. The use according to claim 1, characterized in that: In the step (1), the concentration of the hydrochloric acid solution is 2-15wt%; in the step (2), the crystallization temperature is 110-170°C and the time is 12-48h; in the step (3), the high temperature calcination temperature is 540-560°C and the time is 1.5-2.5h.

8. The use according to claim 7, characterized in that: In the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g: 1-2 L.

9. The use according to claim 7, characterized in that: In the step (3), the heating rate of the high temperature calcination is 2-5°C / min.

10. The use according to claim 7, characterized in that: In the step (1), the ratio of the rice husk powder to the hydrochloric acid solution is 50-80 g: 1-2 L; in the step (3), the heating rate of the high temperature calcination is 2-5° C. / min.

Citation Information

Patent Citations

  • Method for preparing multistage duct zeolite molecular sieve from rice husk

    CN105731485A

  • Method for preparing hierarchical porous Y-type molecular sieve by using rice husk as raw material

    CN108249456A

  • Method for preparing porous molecular sieve by using unroasted rice hull as template

    CN116177562A

  • AU2020101871A4