Steel-based glass ceramic composite bulletproof material and preparation method thereof

By pouring glass melt onto a steel base and subjecting it to temperature-controlled heat treatment, a glass-ceramic composite material is formed, which solves the problems of heavy weight, high cost, and complex processes of bulletproof armor materials, and achieves lightweight, efficient, and economical bulletproof effects.

CN118851545AActive Publication Date: 2024-10-29WUHAN UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410754504.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-29
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Existing bulletproof armor materials are heavy, have high production costs, and have complex preparation processes, which limit their wide application in military equipment.

Method used

The pouring method is used to pour magnesium-aluminum-silicon, lithium-aluminum-silicon or barium-aluminum-silicon glass melt into the steel base, and then form microcrystalline glass through temperature-controlled heat treatment, which simplifies the preparation process and improves the yield and ballistic resistance.

Benefits of technology

It has realized the preparation of lightweight and economical bulletproof materials, with high bulletproof effect, low weight, customizable production and convenient assembly, which significantly improves the tactical performance of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851545A_ABST
    Figure CN118851545A_ABST
Patent Text Reader

Abstract

The invention discloses a steel-based glass ceramic composite bulletproof material and a preparation method thereof, and belongs to the technical field of functional materials.The preparation method comprises the steps that glass melt of a specific system is accurately poured into a groove structure of a steel-based substrate designed and manufactured in advance through a pouring method, and then the bulletproof material is obtained through a programmed temperature control heat treatment process; the glass melt in the substrate is subjected to nucleation and crystallization to form a glass ceramic layer with excellent physical properties, so that the steel-based glass ceramic composite bulletproof material is prepared. The composite bulletproof material prepared by the invention not only has excellent bulletproof performance, but also realizes light weight of the material due to the addition of the microcrystalline glass. When in use, the bulletproof material is simple, convenient and rapid to assemble, can be conveniently disassembled and maintained when not in use, and even can be stored in a classified manner as required. Due to the characteristics, the composite bulletproof material has a wide application prospect in the field of military protection, and a more efficient and economical protection solution can be provided for modern military equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and specifically relates to a steel-based microcrystalline glass composite bulletproof material and a preparation method thereof. Background Art

[0002] In the research and application of bulletproof armor materials, steel materials have always been the mainstream choice. From traditional ordinary steel armor, to high-hardness steel armor, double-hardness steel composite armor, to advanced titanium alloy armor, its protective performance has been continuously improved. These metal armors play a vital protective role in military equipment such as tanks, armored vehicles, and warships. However, due to its heavy weight, it may affect the tactical performance of the equipment. In recent years, with the development of materials science, the research and application of ceramic materials in the field of bulletproof has gradually increased. Ceramic materials have shown many excellent properties such as high hardness, high compressive strength and good wear resistance due to their unique physical and chemical properties. Despite this, the preparation process of ceramic bulletproof armor is relatively complex, the molding difficulty is high and the cost is expensive. These factors limit its wide application in the field of bulletproof.

[0003] Patent CN107388899B discloses a method for preparing a lightweight composite bulletproof plate, which is formed by stacking multiple layers of bulletproof substrates through hot pressing molding technology, wherein the substrate is a steel mesh plate, and its outer surface is sequentially covered with an aluminum layer and a ceramic layer, the aluminum layer is prepared by a hot dip plating process, and the ceramic layer is formed by a micro-arc oxidation process. Although this material has made certain progress in lightweighting, its preparation process is relatively complicated, the process requirements are high, and there are deficiencies in the firmness of the structure, and it is easy to suffer large-scale damage when attacked. Patent CN1746609B provides a steel honeycomb ceramic sandwich composite bulletproof armor plate and a preparation method thereof, which is composed of a metal plate surface, a honeycomb core plate, a ceramic chip and a metal back, and each layer is bonded together by an organic glue layer and a metal brazing layer. However, the bonding strength between the microcrystalline glass chip and the metal is relatively low, and the complexity of the manufacturing process and the high requirements for manufacturing technology have led to an increase in its production cost, which is not conducive to large-scale production and application.

[0004] In view of the limitations of the prior art, the present invention aims to provide a new type of steel-based microcrystalline glass composite bulletproof material and a preparation method thereof, aiming to overcome the problems of weight, cost and preparation process in the prior art, so as to achieve a more efficient and economical bulletproof armor solution. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a steel-based microcrystalline glass composite bulletproof material.

[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: comprising:

[0009] The glass components are melted to form a glass melt, which is then poured into a steel base substrate using a casting method, and subjected to temperature-controlled heat treatment to obtain microcrystalline glass. After post-treatment, a steel-based microcrystalline glass composite bulletproof material is obtained.

[0010] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the glass component includes one of the magnesium aluminum silicon series, lithium aluminum silicon series, and barium aluminum silicon series glass components.

[0011] As a preferred scheme for the preparation method of the steel-based microcrystalline glass composite bulletproof material described in the present invention, the magnesium-aluminum-silicon glass component includes, by weight percentage, MgO 8-20wt%, Al2O3 15-25wt%, SiO2 50-60wt%, TiO2+ZrO2<8wt%, and B2O3<5wt%.

[0012] As a preferred scheme for the preparation method of the steel-based microcrystalline glass composite bulletproof material described in the present invention, the lithium aluminum silicate glass component includes, by weight percentage, Li2O 2-3wt%, Al2O3 15-30wt%, SiO2 55-75wt%, TiO2+ZrO2<2wt%, and Na2O+K2O<4wt%.

[0013] As a preferred scheme of the preparation method of the steel-based microcrystalline glass composite bulletproof material described in the present invention, wherein: the barium aluminum silicon glass component includes, by weight percentage, BaO 16~24wt%, Al2O315~22wt%, SiO243~54wt%, CaO 0~2wt%, MgO 0~3wt%, TiO2+ZrO2<4wt%, and Na2O+B2O3<4wt%.

[0014] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, wherein: the glass component is a magnesium-aluminum-silicon glass component.

[0015] As a preferred embodiment of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the glass melting temperature used is 1300-1600° C. and the melting time is 1-3 hours.

[0016] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the steel base used is one of 304 stainless steel, manganese 13 steel and ductile iron.

[0017] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the elongation of the steel-based material is 3-20%, the tensile strength is 300-800 MPa, and the Young's modulus is 170-205 GPa.

[0018] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the steel-based material used is a material that can withstand a casting temperature of 1300°C to 1600°C.

[0019] As a preferred scheme for the preparation method of the steel-based microcrystalline glass composite bulletproof material described in the present invention, the steel base used has a groove structure with different shapes, the shape of the groove is a regular quadrangular pyramid or a regular hexagonal pyramid, the upper side length of the prism is 1 to 5 cm, the lower side length is 1 to 5 cm, the height is 2 to 5 cm, the inclination angle of the side of the prism-shaped groove is 1° to 6°, and there is a through hole at the bottom of the groove.

[0020] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the steel base used is prepared from a graphite mold and can be reused, and molds of different shapes can be prepared according to different usage requirements.

[0021] As a preferred solution of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the temperature-controlled heat treatment is a two-step program temperature control.

[0022] As a preferred embodiment of the method for preparing the steel-based microcrystalline glass composite bulletproof material of the present invention, the two-step programmed temperature control is as follows: the magnesium aluminum silicate glass is firstly heat-insulated and nucleated at 730-830°C for 2-4 hours, and then heat-insulated and crystallized at 850-950°C for 1-3 hours; the lithium aluminum silicate glass is firstly heat-insulated and nucleated at 500-600°C for 2-4 hours, and then heat-insulated and crystallized at 620-720°C for 1-3 hours; the barium aluminum silicate glass is firstly heat-insulated and nucleated at 780-880°C for 2-4 hours, and then heat-insulated and crystallized at 900-1000°C for 1-3 hours.

[0023] Beneficial effects of the present invention:

[0024] (1) Simplified preparation process: The present invention adopts a process of directly pouring glass melt onto a prefabricated steel base substrate, and then achieving crystallization through heat treatment, which simplifies the preparation process of the composite material, improves the yield rate, and reduces the manufacturing cost;

[0025] (2) Excellent bulletproof effect: The prepared bulletproof material exhibits excellent resistance to large bullets, artillery shells, reinforced bullets and other highly destructive ammunition, providing a higher level of protection;

[0026] (3) Lightweight design: The density of the bulletproof glass-ceramic material of the present invention is 2.3-3.0 g / cm 3 , Vickers hardness 550 ~ 900HV, steel density 7.7 ~ 8g / cm 3 , Vickers hardness of about 200HV, the density of microcrystalline glass is 1 / 3 of that of steel, but its hardness is nearly 4 times that of steel, so the weight of the bulletproof material of the present invention is reduced to half to one-third compared with ordinary steel armor, high-hardness steel armor, and double-hardness steel composite armor. Under the premise of maintaining the same bulletproof effect, the weight of combat equipment can be significantly reduced, thereby greatly improving the tactical performance of the equipment;

[0027] (4) Advantages of composite structure: The composite structure of the present invention is formed in one step by casting, taking advantage of the difference in thermal expansion coefficients between the steel-based material and the microcrystalline glass, i.e., the thermal expansion coefficient of the steel-based material is 10*10 -6 / K~20*10 -6 / K, the thermal expansion coefficient of glass-ceramics is 3*10 -6 / K~8*10 -6 / K. Therefore, during the cooling process of heat treatment, due to the huge difference in thermal expansion coefficients between the two, the microcrystalline glass is firmly fixed on the steel base and is not easy to fall off. This can give full play to the light weight, high hardness and compressive strength of the microcrystalline glass and the toughness of the steel. The two complement each other, effectively disperse the kinetic energy of the projectile, and enhance the overall strength of the bulletproof module;

[0028] (5) Efficient projectile energy absorption: When a projectile hits, the glass-ceramic plate absorbs the energy in a crushing manner, while the terrace-like structure of the groove helps to disperse the impact force to the surrounding areas. In addition, at the moment of impact, due to the high hardness of the glass-ceramic, the bullet head will be squeezed and deformed, minimizing the destructive power of the projectile, effectively resisting the projectile, and protecting the main body of the equipment from damage;

[0029] (6) Customizable production: According to different usage requirements, composite bulletproof materials of different specifications and shapes can be manufactured by changing the size and shape of the mold, and the mold is reusable, which improves the flexibility and economy of production;

[0030] (7) Convenient assembly and maintenance: The composite bulletproof material of the present invention can be produced in small modules, which is convenient for assembly and the assembly process is simple and fast, which is convenient for rapid deployment. When not in use, it can be easily disassembled for maintenance and classified storage, which solves the problem of difficult assembly and inconvenient maintenance of traditional armor materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0032] Figure 1 This is a schematic diagram of a steel base structure with a regular quadrangular pyramid groove used in the present invention.

[0033] Figure 2 This is a schematic diagram of the cross-sectional structure of a steel base with a regular quadrangular pyramid groove used in the present invention.

[0034] Figure 3 The following are photos of the steel substrate used in the present invention (front and back).

[0035] Figure 4 Comparison photos of the glass prepared in Example 1 before and after microcrystallization.

[0036] Figure 5 This is a photo of the steel-based glass-ceramic composite bullet-proof material prepared in Example 1 after polishing.

[0037] Figure 6 These are front and back photos of the steel-based glass-ceramic composite bullet-proof material prepared in Example 1 after being impacted by a 12.7mm bullet at a distance of 100m.

[0038] Figure 7 These are photos of the front and back sides of the steel-based glass-ceramic composite bullet-proof material prepared in Comparative Example 3 after being impacted by a 12.7mm bullet at a distance of 100m. DETAILED DESCRIPTION

[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0041] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0042] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art.

[0043] The structural schematic diagram of the steel-based material prepared by the present invention is as follows Figure 1 , 2 As shown, the figure marks are: H is the thickness of the steel base; h is the height of the groove; a is the length of the upper side of the groove; b is the length of the lower side of the groove; c is the distance between the upper sides of two adjacent grooves. It can be a groove structure with different shapes, the shape of the groove is a regular quadrangular pyramid or a regular hexagonal pyramid, the upper side length of the prism is 1 to 5 cm, the lower side length is 1 to 5 cm, the height is 2 to 5 cm, the inclination angle of the side of the prism-shaped groove is 1° to 6°, and there is a through hole at the bottom of the groove;

[0044] Specifically, in the embodiments and comparative examples of the present invention, a melt of 304 stainless steel, manganese 13 steel and ductile iron is poured into a pre-made graphite mold to prepare a steel base with a specific geometric shape. Figure 3 As shown, its length and width are both 33.5 cm, the thickness (H) is 5 cm, the upper side length (a) of the groove is 5 cm, the lower side length (b) is 4.5 cm, and the height (h) is 4.5 cm; the groove is in the shape of a regular quadrangular pyramid, the distance between its upper sides (c) is 0.3 cm, and the inclination angle (α) of the side of the pyramid is 3.12°.

[0045] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art.

[0046] Example 1

[0047] In this embodiment, a magnesium-aluminum-silicon glass component is selected to prepare a glass melt, specifically, its composition is MgO 14wt%, Al2O3 20wt%, SiO2 60wt%, TiO2+ZrO2 4wt%, B2O3 2wt%;

[0048] 1) placing the magnesium-aluminum-silicon glass component in a muffle furnace at a temperature of 1550° C. and melting it for 2 hours to form a uniform glass melt;

[0049] 2) Pour the molten glass into the groove of the 304 stainless steel base, and heat the combination of the steel base and the molten glass to 770°C at a heating rate of 5°C / min and keep it for 2 hours; continue to heat it to 900°C and keep it for 2 hours to promote the nucleation and crystallization process of the molten glass;

[0050] 3) After the heat treatment is completed, the material is allowed to cool naturally to room temperature, and the surface of the module board is polished by a machine to make it flat and smooth; a layer of canvas is pasted on the surface using epoxy resin to obtain a steel-based microcrystalline glass composite bulletproof material.

[0051] Figure 4 The following are comparison pictures of the glass batch material before and after microcrystallization in this embodiment. It can be seen that the original transparent glass is transformed into white microcrystal glass after heat treatment, and this change indicates that the microcrystallization of the material is successfully completed.

[0052] Figure 5 This is a photo of the steel-based microcrystalline glass composite bulletproof material prepared in this example. It can be clearly seen from the picture that the microcrystalline glass and the steel base are very tightly bonded, and there is no gap at the interface, which proves that the microcrystalline glass and the steel base have achieved good composite.

[0053] The steel-based microcrystalline glass composite bulletproof material prepared in this embodiment was subjected to an impact test. The impact test method was as follows: at a distance of 100m, a 12.7mm caliber assault rifle was used to shoot at the bulletproof material. Photos of the front and back after impact were as follows: Figure 6 As shown in the figure, it can be seen that an impact crater is formed after the front impact of the bullet-proof material, and a bulge is formed on the back of the bullet-proof material, but it is not penetrated, indicating that the bullet-proof material successfully resists the impact of the bullet.

[0054] Example 2

[0055] The difference between this embodiment and embodiment 1 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is MgO 17wt%, Al2O3 20wt%, SiO2 55wt%, TiO2+ZrO2 5wt%, and B2O3 3wt%. The remaining steps and processes are all referred to embodiment 1 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0056] Example 3

[0057] The difference between this embodiment and embodiment 1 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is MgO 17wt%, Al2O3 25wt%, SiO2 50wt%, TiO2+ZrO2 6wt%, B2O3 2wt%, and the remaining steps and processes are all referred to embodiment 1 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0058] Example 4

[0059] The difference between this embodiment and embodiment 1 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is MgO 12wt%, Al2O3 21wt%, SiO2 60wt%, TiO2+ZrO2 5wt%, and B2O3 2wt%. The remaining steps and processes are all referred to embodiment 1 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0060] The density and thermal expansion coefficient of the glass-ceramics prepared in Examples 1 to 4, as well as the results of the compressive strength test and the impact resistance test of the steel-based glass-ceramics composite bullet-proof materials prepared in Examples 1 to 4 are shown in Table 1.

[0061] Test method for compressive strength of glass-ceramics: Cut the prepared glass-ceramics into blocks of 5*5*5mm and use a universal testing machine to test the compressive strength. The test standard refers to the national standard GB / T 19760-2016 "Glass-ceramics".

[0062] Glass-ceramic density test method: Use an analytical balance with density test to measure the mass of the crystals in air and in anhydrous ethanol, use Archimedes' principle to calculate the volume of the sample, and then find the density. The test standard refers to the national standard GB / T 19760-2016 "Glass-ceramic".

[0063] Vickers hardness test method for glass-ceramics: Prepare glass-ceramics samples into blocks of 10*10*5mm, and polish the surface to make it flat, smooth, and free of obvious defects. Use a Vickers hardness tester to test the hardness. The test standard refers to the national standard GB / T 19760-2016 "Glass-ceramics".

[0064] Test method for thermal expansion coefficient of microcrystalline glass: Cut the prepared microcrystalline glass into blocks of 5*5*30mm, put them into the thermal expansion coefficient tester, and use the ejector method for testing. The test standard refers to the national standard GB / T19760-2016 "Microcrystalline Glass".

[0065] The impact resistance test method is: at a distance of 100m, use an assault rifle with a caliber of 12.7mm to shoot at the bulletproof material. If the bulletproof material cannot be penetrated, it means that it can withstand the impact. If it can penetrate the bulletproof material, it means that it cannot withstand the impact.

[0066] Table 1

[0067] Test Project Example 1 Example 2 Example 3 Example 4 Compressive strength(MPa) 750 732 738 735 <![CDATA[Density of glass-ceramics (g / cm 3 )]]> 2.66 2.68 2.65 2.69 Vickers hardness of glass-ceramics (HV) 773 772 775 774 <![CDATA[Coefficient of thermal expansion of glass-ceramics (10 -6 / K)]]> 6.3 6.5 6.4 6.3 Can it withstand the impact? yes yes yes yes

[0068] As shown in Table 1, the density of magnesium-aluminum-silicon glass-ceramics is between 2.66 and 3 g / cm3 , Vickers hardness is about 773HV, and the density of steel is 7.7~8g / cm 3 , Vickers hardness is about 2GPa, the density of microcrystalline glass is 1 / 3 of that of steel, but its hardness is 3 times that of steel. Therefore, the weight of the bulletproof material of this embodiment is reduced to half to one-third compared with ordinary steel armor, high-hardness steel armor, and double-hardness steel composite armor. Under the premise of maintaining the same bulletproof effect, it can significantly reduce the weight of combat equipment and greatly improve the tactical performance of the equipment.

[0069] As shown in Table 1, the thermal expansion coefficient of magnesium aluminum silicon glass-ceramics is 6.3*10 -6 / K~6.5*10 -6 / K, the thermal expansion coefficient of 304 stainless steel base is 17.3*10 -6 / K or so, using the difference in thermal expansion coefficients between the steel-based material and the microcrystalline glass. That is, during the cooling process of heat treatment, due to the huge difference in thermal expansion coefficients between the two, the microcrystalline glass is firmly fixed on the steel-based substrate and is not easy to fall off.

[0070] It can be seen from Table 1 that in Example 1, when magnesium-aluminum-silicon glass components are selected to prepare a glass melt, and its composition is MgO 14wt%, Al2O3 20wt%, SiO2 60wt%, TiO2+ZrO2 4wt%, and B2O3 2wt%, the compressive strength of the steel-based microcrystalline glass composite bullet-proof material prepared is the largest, reaching 750MPa, indicating that when a 304 stainless steel base is used, the steel-based microcrystalline glass composite material formed by the microcrystalline glass of this composition can withstand impact and has high strength as a bullet-proof material.

[0071] Example 5

[0072] In this embodiment, a lithium aluminum silicon glass component is selected to prepare a glass melt, specifically, its composition is Li2O3wt%, Al2O320wt%, SiO275wt%, TiO2+ZrO21wt%, Na2O+K2O 1wt%;

[0073] 1) placing the lithium aluminum silicon glass component in a muffle furnace at a temperature of 1350° C. and melting for 2 hours to form a uniform glass melt;

[0074] 2) Pour the molten glass into the groove of the 304 stainless steel base, and heat the combination of the steel base and the molten glass to 540°C at a heating rate of 5°C / min and keep it for 2 hours; continue to heat it to 650°C and keep it for 2 hours to promote the nucleation and crystallization process of the molten glass;

[0075] 3) After the heat treatment is completed, the material is allowed to cool naturally to room temperature, and the surface of the module board is polished by a machine to make it flat and smooth; a layer of canvas is pasted on the surface using epoxy resin to obtain a steel-based microcrystalline glass composite bulletproof material.

[0076] Example 6

[0077] The difference between this embodiment and embodiment 5 is that the proportions of the components in the lithium aluminum silicon glass component are different. Specifically, the composition is Li2O 2wt%, Al2O3 25wt%, SiO2 70wt%, TiO2+ZrO2 1wt%, Na2O+K2O 2wt%, and the remaining steps and processes are all referred to embodiment 5 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0078] Example 7

[0079] The difference between this embodiment and embodiment 5 is that the proportions of the components in the lithium aluminum silicon glass component are different. Specifically, the components are Li2O 3wt%, Al2O3 28wt%, SiO2 65wt%, TiO2+ZrO2 1.5wt%, Na2O+K2O 3.5wt%. The remaining steps and processes are all based on embodiment 5 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0080] The density and thermal expansion coefficient of the microcrystalline glass prepared in Examples 5 to 7, as well as the compressive strength test and impact resistance test of the steel-based microcrystalline glass composite bullet-proof materials prepared in Examples 5 to 7 were compared with those in Example 1. The results are shown in Table 2.

[0081] Table 2

[0082] Test Project Example 1 Example 5 Example 6 Example 7 Compressive strength(MPa) 750 693 682 689 <![CDATA[Density of glass-ceramics (g / cm 3 )]]> 2.66 2.44 2.46 2.45 Vickers hardness of glass-ceramics (HV) 773 725 731 727 <![CDATA[Coefficient of thermal expansion of glass-ceramics (10 -6 / K)]]> 6.3 5.1 4.9 5.0 Can it withstand the impact? yes yes yes yes

[0083] As shown in Table 2, the density of lithium aluminum silicon glass-ceramics is 2.44-2.46 g / cm 3 , Vickers hardness is about 728HV.

[0084] As shown in Table 2, the thermal expansion coefficient of lithium aluminum silicon glass-ceramics is 4.9*10 -6 / K~5.1*10 -6 / K, can be firmly fixed on the steel base.

[0085] It can be seen from Table 2 that when the steel base is not changed and only the glass component is adjusted to a lithium aluminum silicon glass component, the compressive strength of the steel-based microcrystalline glass composite bullet-proof material prepared in Example 5, i.e., the composition is Li2O 3wt%, Al2O3 20wt%, SiO2 75wt%, TiO2+ZrO2 1wt%, and Na2O+K2O 1wt%, is the largest, which is 693MPa, but is still less than the steel-based microcrystalline glass composite bullet-proof material prepared when the magnesium aluminum silicon glass component is selected in Example 1.

[0086] Example 8

[0087] In this embodiment, a barium aluminum silicon glass component is selected to prepare a glass melt, specifically, its composition is BaO20wt%, Al2O318wt%, SiO254wt%, CaO 2wt%, MgO 3wt%, TiO2+ZrO21wt%, Na2O+B2O32wt%;

[0088] 1) Place the barium aluminum silicon glass component in a muffle furnace at a temperature of 1600°C and melt for 2 hours to form a uniform glass melt;

[0089] 2) Pour the melted glass melt into the groove of the 304 stainless steel base; heat the combination of the steel base and the glass melt to 820°C at a heating rate of 5°C / min and keep it for 2 hours; continue to heat it to 950°C and keep it for 2 hours to promote the nucleation and crystallization process of the glass melt;

[0090] 3) After the heat treatment is completed, the material is allowed to cool naturally to room temperature, and the surface of the module board is polished by a machine to make it flat and smooth; a layer of canvas is pasted on the surface using epoxy resin to obtain a steel-based microcrystalline glass composite bulletproof material.

[0091] Example 9

[0092] The difference between this embodiment and Embodiment 8 is that the proportions of the components in the barium aluminum silicon glass component are different. Specifically, the composition is BaO 20wt%, Al2O3 20wt%, SiO2 50wt%, CaO 2wt%, MgO 3wt%, TiO2+ZrO2 3wt%, Na2O+B2O3 2wt%. The remaining steps and processes are all referred to Embodiment 8 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0093] Example 10

[0094] The difference between this embodiment and Embodiment 8 is that the proportions of the components in the barium aluminum silicon glass component are different. Specifically, the composition is BaO 18wt%, Al2O3 20wt%, SiO2 54wt%, CaO 2wt%, MgO 3wt%, TiO2+ZrO2 1wt%, Na2O+B2O3 2wt%. The remaining steps and processes are all referred to Embodiment 8 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0095] The density and thermal expansion coefficient of the microcrystalline glass prepared in Examples 8 to 10, as well as the compressive strength test and impact resistance test of the steel-based microcrystalline glass composite bullet-proof materials prepared in Examples 8 to 10 were compared with those in Example 1. The results are shown in Table 3.

[0096] Table 3

[0097] Test Project Example 1 Example 8 Example 9 Example 10 Compressive strength(MPa) 750 663 654 652 <![CDATA[Density of glass-ceramics (g / cm 3 )]]> 2.66 2.73 2.75 2.76 Vickers hardness of glass-ceramics (HV) 773 765 760 766 <![CDATA[Coefficient of thermal expansion of glass-ceramics (10 -6 / K)]]> 6.3 7.1 7.3 7.2 Can it withstand the impact? yes yes yes yes

[0098] As shown in Table 3, the density of barium aluminum silicon glass-ceramics is between 2.73 and 2.76 g / cm 3 , Vickers hardness is about 764HV.

[0099] As shown in Table 3, the thermal expansion coefficient of barium aluminum silicon glass-ceramics is 7.1*10 -6 / K~7.3*10 -6 / K, can be firmly fixed on the steel base.

[0100] It can be seen from Table 3 that when the steel base is not changed and only the glass component is adjusted to a lithium aluminum silicon glass component, the compressive strength of the steel-based microcrystalline glass composite bullet-proof material prepared in Example 8, i.e., the composition is BaO 20wt%, Al2O3 18wt%, SiO2 54wt%, CaO 2wt%, MgO 3wt%, TiO2+ZrO2 1wt%, and Na2O+B2O3 2wt%, is the maximum, which is 663MPa, but is less than the steel-based microcrystalline glass composite bullet-proof material prepared when the magnesium aluminum silicon glass component is selected in Example 1.

[0101] It can be seen from the results in Tables 1 to 3 that when the steel-based structure is unified, the overall compressive strength of the steel-based glass-ceramic composite bullet-proof material using magnesium-aluminum-silicon glass-ceramics is greater than that of lithium-aluminum-silicon glass-ceramics and greater than that of barium-aluminum-silicon glass-ceramics.

[0102] Embodiment 11

[0103] The difference between this embodiment and embodiment 1 is that the steel base used in step (2) is different and is adjusted to a manganese 13 steel base, and the remaining steps and processes are all referred to embodiment 1 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0104] Example 12

[0105] The difference between this embodiment and embodiment 5 is that the steel base used in step (2) is different and is adjusted to a manganese 13 steel base, and the remaining steps and processes are all referred to embodiment 5 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0106] Embodiment 13

[0107] The difference between this embodiment and embodiment 8 is that the steel base used in step (2) is different and is adjusted to a manganese 13 steel base. The remaining steps and processes are all based on embodiment 8 to obtain the steel-based microcrystalline glass composite bulletproof material of this embodiment.

[0108] The density and thermal expansion coefficient of the microcrystalline glass prepared in Examples 11 to 13, as well as the compressive strength test and impact resistance test of the steel-based microcrystalline glass composite bullet-proof materials prepared in Examples 11 to 13 were compared with those in Example 1. The results are shown in Table 4.

[0109] Table 4

[0110] Test Project Example 1 Embodiment 11 Example 12 Embodiment 13 Compressive strength(MPa) 750 745 684 667 <![CDATA[Density of glass-ceramics (g / cm 3 )]]> 2.66 2.65 2.45 2.74 Vickers hardness of glass-ceramics (HV) 773 774 736 764 <![CDATA[Coefficient of thermal expansion of glass-ceramics (10 -6 / K)]]> 6.3 6.3 5.0 7.1 Can it withstand the impact? yes yes yes yes

[0111] As shown in Table 4, the thermal expansion coefficient of glass-ceramics is 5.0*10 -6 / K~7.1*10 -6 / K, the thermal expansion coefficient of manganese 13 steel base is 12*10 -6 / K, the microcrystalline glass can be fixed on the steel base.

[0112] It can be seen from Table 4 that when the steel base type is adjusted to manganese 13 steel base, the steel-based microcrystalline glass composite bullet-proof material prepared using magnesium aluminum silicon glass components exhibits the strongest compressive strength, reaching 745 MPa, but is still lower than the steel-based microcrystalline glass composite bullet-proof material prepared when stainless steel is selected as the steel base in Example 1.

[0113] Comparative Example 1

[0114] The difference between this comparative example and Example 1 is that the steel base used in step (2) is different and is adjusted to a ductile iron steel base, and the remaining steps and processes are all referred to Example 1 to obtain the steel-based microcrystalline glass composite bulletproof material of this comparative example.

[0115] Comparative Example 2

[0116] The difference between this comparative example and Example 5 is that the steel base used in step (2) is different and is adjusted to a ductile iron steel base, and the remaining steps and processes are all referred to Example 5 to obtain the steel-based microcrystalline glass composite bulletproof material of this comparative example.

[0117] Comparative Example 3

[0118] The difference between this comparative example and Example 8 is that the steel base used in step (2) is different and is adjusted to a ductile iron steel base, and the remaining steps and processes are all referred to Example 8 to obtain the steel-based microcrystalline glass composite bulletproof material of this comparative example.

[0119] Figure 7 The front and back photos of the steel-based microcrystalline glass composite bulletproof material prepared in this comparative example after being impacted by a 12.7mm bullet at a distance of 100m. From the pictures, it can be seen that a large impact crater is formed after the front impact of the bulletproof material, and the back of the bulletproof material is penetrated by the bullet. This shows that the bulletproof material prepared in this comparative example cannot withstand the impact of the bullet.

[0120] The density and thermal expansion coefficient of the microcrystalline glass prepared in Comparative Examples 1 to 3, as well as the compressive strength test and impact resistance test of the steel-based microcrystalline glass composite bullet-proof materials prepared in Comparative Examples 1 to 3 were compared with Example 1. The results are shown in Table 5.

[0121] Table 5

[0122] Test Project Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Compressive strength(MPa) 750 747 685 662 <![CDATA[Density of glass-ceramics (g / cm 3 )]]> 2.66 2.65 2.44 2.74 Vickers hardness of glass-ceramics (HV) 773 771 736 767 <![CDATA[Coefficient of thermal expansion of glass-ceramics (10 -6 / K)]]> 6.3 6.2 5.0 7.2 Can it withstand the impact? yes yes no no

[0123] As shown in Table 5, the thermal expansion coefficient of glass-ceramics is 5.0*10 -6 / K~7.2*10 -6 / K, the thermal expansion coefficient of ductile iron steel base is 11.2*10 -6 / K or so, the microcrystalline glass can be firmly fixed on the steel base.

[0124] It can be seen from Table 5 that when the steel base type is adjusted to ductile iron steel base, the steel-based microcrystalline glass composite bullet-proof material prepared using the magnesium-aluminum-silicon glass component exhibits the strongest compressive strength, reaching 747 MPa, but is still less than the steel-based microcrystalline glass composite bullet-proof material prepared when stainless steel is selected as the steel base in Example 1.

[0125] It can also be seen from Table 5 that only the steel-based microcrystalline glass composite bulletproof material prepared using magnesium-aluminum-silicon glass components can withstand impact and have bulletproof performance, that is, when ductile iron is used as the steel base, it can withstand impact when combined with magnesium-aluminum-silicon microcrystalline glass with relatively high compressive strength, but cannot withstand the impact of a 12.7mm bullet at a distance of 100m when combined with lithium-aluminum-silicon and barium-aluminum-silicon microcrystalline glass with relatively low compressive strength. This is because ductile iron has low strength and contains non-spherical graphite forms, which reduces its deformation and plastic deformation capabilities during heat treatment. When the compressive strength of the microcrystalline glass is low, the ductile iron is prone to cracking after being impacted by a bullet and cannot withstand the impact of the bullet.

[0126] Comparative Example 4

[0127] The difference between this comparative example and comparative example 1 is that the two-step heat treatment temperatures are different. In this comparative example, the combination of the steel base and the glass melt is heated to 700°C at a heating rate of 5°C / min and maintained for 2 hours; the temperature is further raised to 800°C and maintained for 2 hours; the remaining steps are all referred to comparative example 1, and the ductile iron steel-based magnesium-aluminum-silicon glass composite bullet-proof material of this comparative example is obtained.

[0128] Comparative Example 5

[0129] The difference between this comparative example and comparative example 1 is that the two-step heat treatment temperatures are different. In this comparative example, the combination of the steel base and the glass melt is heated to 850°C at a heating rate of 5°C / min and maintained for 2 hours; the temperature is further raised to 980°C and maintained for 2 hours; the remaining steps are all referred to comparative example 1, and the ductile iron steel-based magnesium-aluminum-silicon glass composite bullet-proof material of this comparative example is obtained.

[0130] Comparative Example 6

[0131] The difference between this comparative example and comparative example 1 is that the two-step heat treatment time is different. In this comparative example, the combination of the steel base and the glass melt is heated to 770°C at a heating rate of 5°C / min and maintained for 1 hour; the temperature is further raised to 900°C and maintained for 1 hour; the remaining steps are all referred to comparative example 1 to obtain the ductile iron steel-based magnesium-aluminum-silicon glass composite bullet-proof material of this comparative example.

[0132] The density and thermal expansion coefficient of the glasses prepared in Comparative Examples 4 to 6, as well as the compressive strength test and impact resistance test of the glass composite bullet-proof materials prepared in Comparative Examples 4 to 6 were compared with those in Example 1. The results are shown in Table 6.

[0133] Table 6

[0134] Test Project Example 1 Comparative Example 4 Comparative Example 5 Comparative Example 6 Compressive strength(MPa) 750 279 205 479 Can it withstand the impact? yes no no no

[0135] It can be seen from Table 6 that when preparing magnesium-aluminum-silicon glass-ceramics, when the heat treatment temperature is too low or too high, or the heat treatment time is too short, the degree of crystallization of the glass will be reduced or it will not be able to crystallize at all, resulting in extremely low compressive strength of the glass, which cannot withstand the impact of a 12.7mm bullet at a distance of 100m.

[0136] Comparative Example 7

[0137] The difference between this comparative example and Example 1 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is adjusted to MgO 14wt%, Al2O3 20wt%, SiO2 60wt%, CaO 2wt%, B2O3 2wt%, P2O 52wt%, and the remaining steps and processes are all referred to Example 1 to obtain the 304 stainless steel-based magnesium-aluminum-silicon glass composite bullet-proof material of this comparative example.

[0138] Comparative Example 8

[0139] The difference between this comparative example and Example 11 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is adjusted to MgO 14wt%, Al2O3 20wt%, SiO2 60wt%, CaO 2wt%, B2O3 2wt%, P2O 52wt%, and the remaining steps and processes are referred to Example 11 to obtain the manganese 13 steel-based magnesium-aluminum-silicon glass composite bulletproof material of this comparative example.

[0140] Comparative Example 9

[0141] The difference between this comparative example and comparative example 1 is that the proportions of the components in the magnesium-aluminum-silicon glass component are different. Specifically, the composition is adjusted to MgO 14wt%, Al2O3 20wt%, SiO2 60wt%, CaO 2wt%, B2O3 2wt%, P2O 52wt%, and the remaining steps and processes are all referred to comparative example 1 to obtain the ductile iron steel-based magnesium-aluminum-silicon glass composite bullet-proof material of this comparative example.

[0142] The density and thermal expansion coefficient of the glasses prepared in Comparative Examples 7 to 9, as well as the compressive strength test and impact resistance test of the glass composite bullet-proof materials prepared in Comparative Examples 7 to 9, were compared with those in Example 1. The results are shown in Table 7.

[0143] Table 7

[0144] Test Project Example 1 Comparative Example 4 Comparative Example 5 Comparative Example 6 Compressive strength(MPa) 750 178 175 176 Can it withstand the impact? yes no no no

[0145] It can be seen from Table 7 that when using magnesium-aluminum-silicon common glass, when combined with 304 stainless steel, manganese 13 steel and ductile iron steel base, it cannot withstand the impact of a 12.7mm bullet at a distance of 100m. This is because the glass prepared under this magnesium-aluminum-silicon glass composition is ordinary glass rather than microcrystalline glass. Ordinary glass cannot be microcrystallized during heat treatment, and its compressive strength is much lower than that of magnesium-aluminum-silicon microcrystalline glass, so it cannot withstand the impact of bullets.

[0146] In summary, the present invention provides a steel-based microcrystalline glass composite bulletproof material and a preparation method thereof, wherein a glass melt of a magnesium-aluminum-silicon glass component is precisely cast into a groove structure of a pre-designed and manufactured steel-based substrate by a casting method and the component ratio is optimized, and then a programmed temperature-controlled heat treatment process is performed so that the glass melt in the substrate undergoes nucleation and crystallization to form a microcrystalline glass layer with excellent physical properties, thereby obtaining a steel-based microcrystalline glass composite bulletproof material with a tight bond and seamless interface, and this material can avoid being penetrated when impacted by a 12.7mm bullet at a distance of 100m, reflecting the bulletproof effect of the steel-based microcrystalline glass composite material.

[0147] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a steel-based glass-ceramic composite bulletproof material, characterized in that: include, The glass components are melted to form a glass melt, which is then poured into a steel base substrate using a casting method, and subjected to temperature-controlled heat treatment to obtain glass-ceramics. After post-treatment, a steel-based glass-ceramics composite bullet-proof material is obtained.

2. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 1, characterized in that: The glass component includes one of magnesium aluminum silicon series, lithium aluminum silicon series, and barium aluminum silicon series glass components.

3. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 2, characterized in that: The magnesium-aluminum-silicon glass components include, by weight percentage, MgO 8-20wt%, Al2O3 15-25wt%, SiO2 50-60wt%, TiO2+ZrO2<8wt%, and B2O3<5wt%.

4. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 2, characterized in that: The lithium aluminum silicate glass components include, by weight percentage, Li2O 2-3wt%, Al2O3 15-30wt%, SiO2 55-75wt%, TiO2+ZrO2<2wt%, and Na2O+K2O<4wt%.

5. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 2, characterized in that: The barium aluminum silicate glass components include, by weight percentage, BaO 16-24wt%, Al2O3 15-22wt%, SiO2 43-54wt%, CaO 0-2wt%, MgO 0-3wt%, TiO2+ZrO2<4wt%, and Na2O+B2O3<4wt%.

6. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 1, characterized in that: The glass component is a magnesium-aluminum-silicon glass component.

7. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 1, characterized in that: The melting temperature of the glass melt is 1300-1600° C., and the melting time is 1-3 hours.

8. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 1, characterized in that: The steel base includes one of 304 stainless steel, manganese 13 steel and ductile iron.

9. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 1, characterized in that: The temperature-controlled heat treatment is a two-step temperature-controlled process.

10. The method for preparing the steel-based glass-ceramic composite bulletproof material according to claim 9, characterized in that: The two-step program temperature control is as follows: the magnesium aluminum silicate glass is firstly heat-insulated and nucleated at 730-830°C for 2-4 hours, and then heat-insulated and crystallized at 850-950°C for 1-3 hours; the lithium aluminum silicate glass is firstly heat-insulated and nucleated at 500-600°C for 2-4 hours, and then heat-insulated and crystallized at 620-720°C for 1-3 hours; the barium aluminum silicate glass is firstly heat-insulated and nucleated at 780-880°C for 2-4 hours, and then heat-insulated and crystallized at 900-1000°C for 1-3 hours.

Citation Information

Patent Citations

  • Corrugated microcrystalline glass and preparation method thereof

    CN105293933A

  • Frame glass prepared through medium-high frequency induction heating and preparation method thereof

    CN106565114A

  • High strength glass-ceramics having petalite and lithium silicate structures

    CN110510881A

  • Processing technology for improving glass strength

    CN114105450A

  • Poly-crystalline compositions

    US20050268656A1