Oxide near-infrared luminescent glass ceramic material and preparation method thereof

By preparing oxide near-infrared luminescent glass ceramic materials, the problems of luminous efficiency and service life of near-infrared light sources in the existing technology are solved, and efficient blue light absorption and emission are achieved, which is suitable for industrial production.

CN118851574AActive Publication Date: 2024-10-29JIANGXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410875120.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

Existing near-infrared light sources cannot meet actual needs in terms of luminous efficiency and emission bandwidth. The absorption efficiency of Cr3+ ions is generally lower than 50%. The low thermal conductivity of traditional phosphor-converted LEDs leads to reduced luminous performance and short service life of the device.

Method used

An oxide near-infrared luminescent glass ceramic material is used, with the chemical formula AmBnCpD5O14:xCr3+,yLn3+. It is prepared through high-temperature calcination, melting and amorphous crystallization methods to improve the blue light absorption efficiency and heat dissipation performance of Cr3+ ions. The material has a blue light emission of 430-470nm. The emission wavelength range under excitation is 650-1300nm.

Benefits of technology

It significantly improves the absorption efficiency of blue light from 20.1% to 43.4%, enhances the emission efficiency of near-infrared, extends the service life of LED, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851574A_ABST
    Figure CN118851574A_ABST
Patent Text Reader

Abstract

The invention discloses an oxide near-infrared luminescent glass ceramic material and a preparation method thereof. The general formula of the glass ceramic material is AmBnCpD5O14: xCr < 3 + >, yLn < 3 + >, wherein A is one or a combination of more than two of alkali metals such as Li, Na, K, Rb and Cs; b is one or a combination of more than two of Mg, Ca, Sr, Ba and Zn elements; c is one or a combination of more than two of Al, Ga, Fe, Nb, Ta and rare earth elements; d is one or a combination of more than two of Ti, Si, Ge, Zr, Sn and Hf elements; and Ln is one or more of Yb, Nd, Pr, Eu, Dy and Sm rare earth ions. 0 < = m < = 2.5, 1 < = n < = 4, 0.5 < = p < = 1.5, 0lt; 0 < = y < = 0.5; the glass ceramic is prepared by melting and cooling the fluorescent powder and performing subsequent crystallization heat treatment. The obtained near-infrared luminescent glass ceramic can be efficiently excited by blue light and red light, the emission peak wavelength covers 650-1500nm, the quantum efficiency is higher than that of fluorescent powder, and the near-infrared luminescent glass ceramic can be applied to high-power LED illumination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to an oxide infrared luminescent glass ceramic material and a preparation method thereof. Background Art

[0002] Near-infrared light has shown great application prospects in many fields, including plant growth, non-destructive testing of food analysis, night vision lighting, biological imaging, etc. However, the existing near-infrared light sources still cannot meet the actual needs in terms of luminous efficiency and emission bandwidth. Therefore, the development of new broadband near-infrared light sources has become one of the research focuses of scholars at home and abroad. Among many design schemes, near-infrared phosphor conversion LEDs have shown excellent characteristics, including emission peak position, spectral bandwidth, luminous efficiency and thermal stability. In addition, this scheme has the advantages of simple structure, adjustable spectrum, green and safe preparation method, low cost, and easy miniaturization. Therefore, near-infrared phosphor conversion LEDs are considered to be one of the most reliable broadband near-infrared light source solutions and are expected to be used with portable devices such as mobile phones.

[0003] In recent years, a large number of active ions that emit near-infrared light have been developed, including transition metal ions (such as Mn 2+ 、Ni 2+ , Fe 3+ Cr 4+ and Mn 5+ ) and rare earth ions (such as Pr 3+ 、Nd 3+ 、Tm 3+ , Er 3+ and Yb 3+ ). However, most of these ions have low efficiency, weak absorption, narrow emission spectra, and cannot be excited by blue light. In several studies on near-infrared luminescent materials, Cr 3+ ion should be the best activating ion because it has a unique 3d 3 The electron configuration is conducive to spin prohibition ( 2 E→ 4 A2, 695nm) and spin-allowed ( 4 T2→ 4 A2, 700-1100nm) transition, which matches the low-cost silicon-based photodetector. 3+ The excitation band of the ion ( 4 A2→ 4 T2, 400-500nm) matches the emission wavelength of low-cost commercial blue LED chips well, making Cr 3+ Ions can be efficiently excited by blue light and have great application prospects.

[0004] At present, Cr 3+The internal quantum efficiency of ion-doped near-infrared phosphors can reach nearly 100%, but due to the 3+ The dd parity forbidden transition of ions results in their absorption efficiency generally being less than 50%. To solve this problem, an effective way is to prepare glass ceramics or transparent ceramics, which can reduce the scattering of blue light in the phosphor and enhance the absorption of Cr. 3+ The absorption efficiency of ion-doped near-infrared phosphor in blue light is higher. At the same time, the traditional phosphor-converted LED (pc-LED) needs to be encapsulated by mixing phosphor and solidified colloid. Due to its low thermal conductivity, long-term operation will not only reduce the luminous performance of the device, but also reduce the service life of the LED. Therefore, by directly encapsulating the blue light LED with glass ceramic or transparent ceramic, it can not only improve the Cr 3+ The absorption efficiency of ions in blue light can also improve its heat dissipation performance and service life. However, the existing conditions and methods for preparing glass ceramics or transparent ceramics are harsh, and the luminescence performance is not enough for large-scale application. Therefore, the development of high-performance chromium-doped glass ceramics or transparent ceramics is of great significance for near-infrared light source equipment and applications. Summary of the invention

[0005] The present invention overcomes the shortcomings of the prior art and provides a simple and universal method for preparing glass ceramics. Compared with powders and glass, the blue light absorption efficiency of glass ceramics is greatly improved. Under the excitation of a blue light chip, the emission wavelength is between 650-1300nm, which can be applied to plant lighting, full-spectrum lighting, biological imaging, night vision and other fields.

[0006] The purpose of the present invention is achieved by at least one of the following technical solutions.

[0007] An oxide near-infrared luminescent glass-ceramic material comprising an inorganic compound having a chemical formula of A m B n C p D5O 14 :xCr 3+ ,yLn 3+ ;

[0008] A is one or a combination of two or more of the alkali metals Li, Na, K, Rb and Cs;

[0009] B is one or a combination of two or more of the elements Mg, Ca, Sr, Ba and Zn;

[0010] C is one or a combination of two or more of Al, Ga, In, Fe, Nb, Ta and rare earth elements;

[0011] D is one or a combination of two or more of the elements Ti, Si, Ge, Zr, Sn and Hf;

[0012] O is oxygen element;

[0013] Ln is one or more rare earth elements selected from Yb, Nd, Pr, Eu, Dy and Sm.

[0014] Cr 3+ is the luminescent central ion, Ln 3+ is a sensitizing ion, where 0≤m≤2.5, 1≤n≤4, 0≤p≤1.5, 0% <x≤100%,0%≤y≤20%;

[0015] Preferably, the luminescent glass ceramic material, under the excitation of 430-470nm blue light, has an emission wavelength range of 650-1300nm, a peak value of about 680-100nm, and a half-peak width of up to 100-300nm.

[0016] Preferably, by changing the annealing time and temperature of the material, the blue light absorption efficiency of the material can be increased from 20.1% to 43.4%.

[0017] The preparation method of the above-mentioned oxide near-infrared glass ceramics comprises the following steps:

[0018] 1) According to the chemical formula A m B n C p D5O 14 :xCr 3+ ,yLn 3+ Weigh compound raw materials containing each element in a stoichiometric ratio, grind and mix them to obtain a raw material mixture;

[0019] 2) calcining the mixture obtained in step 1) at high temperature, cooling it to room temperature, and then grinding and sieving it to obtain a powder material;

[0020] 3) melting the powder material obtained in step 2) at high temperature, cooling and annealing to obtain a glass precursor;

[0021] 4) The glass precursor obtained in step 3) is crystallized in an air atmosphere by an amorphous crystallization method, and then the crystallized material is post-processed to obtain the oxide near-infrared glass ceramic.

[0022] Preferably, in step 1), the raw material is a single substance, oxide, halide, sulfide, carbonate, borate, sulfate, phosphate or nitrate of calcium, strontium, barium, lanthanum, neodymium, praseodymium, gallium, aluminum, titanium, tin, germanium, niobium, tantalum and chromium.

[0023] Preferably, in step 1), the grinding time is 5-60 min.

[0024] Preferably, in step 2), the high-temperature calcination is carried out in air or an inert atmosphere, the calcination temperature is 1000-1400° C., and the calcination time is 1-24 h.

[0025] Preferably, in step 3), the melting temperature is 1300-1600° C., and the melting time is 0.2-4 h; the annealing temperature is 450-600° C., and the annealing time is 3-10 h.

[0026] Preferably, in step 4), the amorphous crystallization method is thermal crystallization, the crystallization temperature is 650-1000°C, and the crystallization time is 1-24h; the post-treatment includes polishing with 180 mesh, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh sandpaper respectively, and then polishing with polishing powder, washing and drying.

[0027] The present invention has the following beneficial effects:

[0028] Compared with phosphors, the absorption efficiency of glass ceramics for blue light is increased from 20.1% to 43.1%, which improves the emission efficiency of near-infrared.

[0029] Avoid using resin packaging when packaging devices, change the packaging method of LEDs, and avoid large amounts of heat accumulation in the device that may lead to a decrease in luminous performance.

[0030] The method for making fluorescent glass ceramics has a simple process and strong repeatability, is suitable for large-scale and batch industrial production, and has better chemical stability, density, thermal conductivity and luminous efficiency than traditional phosphors, and has a significant effect on improving the service life and emission power of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the XRD pattern of the near-infrared glass-ceramics prepared in Examples 1-5;

[0032] Figure 2 are the excitation and emission spectra of the near-infrared glass-ceramic of Example 1;

[0033] Figure 3 It is a quantum yield test spectrum diagram of the near-infrared glass ceramic of Example 1 and the phosphor of Comparative Example 1;

[0034] Figure 4 are the excitation and emission spectra of the near-infrared glass ceramic of Example 7 and Comparative Example 3;

[0035] Figure 5 are the excitation and emission spectra of the near-infrared glass ceramic of Example 8 and Comparative Example 4;

[0036] Figure 6 are the excitation and emission spectra of the near-infrared glass ceramic of Example 9 and Comparative Example 5;

[0037] Figure 7 are the excitation and emission spectra of the near-infrared glass ceramic of Example 10 and Comparative Example 6;

[0038] Figure 8 are the excitation and emission spectra of the near-infrared glass ceramic of Example 11 and Comparative Example 8; DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with specific embodiments and drawings to help understand the content of the present invention.

[0040] Example 1: Sr3MgGe5O 14 :0.01Cr 3+ Preparation of fluorescent glass ceramics

[0041] The chemical composition formula of the near-infrared glass ceramic of this embodiment is Sr3MgGe5O 14 :0.01Cr 3+ According to the stoichiometric ratio of each element in the chemical formula, the high-purity powder raw materials of SrCO3, MgO, GeO2 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and sintered at 1150℃ for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor Sr3MgGe5O 14 :0.01Cr 3+ The prepared phosphor was transferred to an alumina crucible, melted at 1350°C for 30 min in an air atmosphere high temperature reactor, quickly taken out at high temperature and poured into a graphite mold preheated at 600°C, pressed with a steel plate, and then quickly transferred to a 600°C annealing furnace for annealing for about 4 hours. The glass obtained after natural cooling was annealed and crystallized in a 920°C high temperature reactor for 8 hours, and then naturally cooled to obtain Sr3MgGe5O 14 :0.01Cr 3+ Glass ceramics. The XRD and fluorescence spectra of its precursor glass and glass ceramics are as follows: Figure 1 and Figure 2 As shown. Figure 1 It can be seen that the glass ceramics and Sr3MgGe5O 14 The standard card matches perfectly, with almost no extra crystalline phase.

[0042] Example 2-5: Sr3MgGe5O 14 :xCr 3+ Preparation of fluorescent glass ceramics

[0043] The preparation methods of Examples 2-5 refer to Example 1, and the melting temperature and time of the glass precursor are the same as those of Example 1. The chemical composition formula, annealing crystallization temperature, annealing crystallization time, blue light absorption efficiency and internal quantum efficiency are shown in Table 1. The XRD comparison chart of the near-infrared fluorescent glass ceramics prepared in Examples 1-6 and the standard card is shown in Figure 1 From the figure, it can be seen that the main crystalline phase of the prepared glass ceramics is Sr3MgGe5O 14 The Sr3MgGe5O prepared in Examples 1-6 14 :xCr 3+ (x=0.01, 0.02, 0.03) The quantum yield test results of glass ceramics are shown in Table 1.

[0044] Example 6: Sr3ZnGe5O 14 :0.01Cr 3+ Preparation of fluorescent glass ceramics

[0045] The preparation method of Example 6 refers to Example 1, and the melting temperature and time of the glass precursor are the same as those of Example 1. The annealing crystallization temperature, annealing crystallization time, blue light absorption efficiency, internal quantum efficiency and luminescence thermal stability are shown in Table 1.

[0046] Examples 7-10: NaSr2CGe5O 14 :0.07Cr 3+ Preparation of (C=Al,Ga,Sc,In) fluorescent glass ceramics

[0047] The preparation methods of Examples 7-10 refer to Example 1, and the melting temperature and time of the glass precursor are the same as those of Example 1. The chemical composition formula, annealing crystallization temperature, annealing crystallization time, blue light absorption efficiency, internal quantum efficiency and luminescence thermal stability are shown in Table 1.

[0048] Examples 11-12: NaB2ScGe5O 14 :0.07Cr 3+ ,0.05Yb 3+ Preparation of (B=Sr,Ca) Fluorescent Glass Ceramics

[0049] The preparation methods of Examples 12-13 refer to Example 1, and the melting temperature and time of the glass precursor are the same as those of Example 1. The chemical composition formula, annealing crystallization temperature, annealing crystallization time, blue light absorption efficiency, internal quantum efficiency and luminescence thermal stability are shown in Table 1.

[0050] Examples 13-14: ASr2ScGe5O 14 :0.07Cr 3+ ,0.05Yb 3+Preparation of (A=Li,K) fluorescent glass ceramics

[0051] The preparation methods of Examples 13-14 refer to Example 1, and the melting temperature and time of the glass precursor are the same as those of Example 1. The chemical composition formula, annealing crystallization temperature, annealing crystallization time, blue light absorption efficiency, internal quantum efficiency and luminescence thermal stability are shown in Table 1.

[0052] Comparative Example 1: Sr3MgGe5O 14 :0.01Cr 3+ Preparation of phosphor

[0053] The chemical composition formula of the near-infrared phosphor in this comparative example is Sr3MgGe5O 14 :0.01Cr 3+ According to the stoichiometric ratio of each element in the chemical formula, high-purity powder raw materials of SrCO3, MgO, GeO2 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and reacted at 1150°C for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor Sr3MgGe5O 14 :0.01Cr 3+ Its blue light absorption efficiency, internal quantum efficiency and luminescence thermal stability are shown in Table 2.

[0054] Comparative Example 2: Sr3ZnGe5O 14 :0.01Cr 3+ Preparation of phosphor

[0055] The chemical composition formula of the near-infrared phosphor in this comparative example is Sr3MgGe5O 14 :0.01Cr 3+ According to the stoichiometric ratio of each element in the chemical formula, high-purity powder raw materials of SrCO3, ZnO, GeO2 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and reacted at 1150°C for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor Sr3MgGe5O 14 :0.01Cr 3+ Its blue light absorption efficiency, internal and external quantum efficiency and luminescence thermal stability are shown in Table 2.

[0056] Comparative Examples 3-6: NaSr2CGe5O 14 :0.07Cr 3+ Preparation of (C=Al,Ga,Sc,In) phosphor

[0057] According to the stoichiometric ratio of each element in the chemical formula, high-purity powder raw materials of Na2CO3, SrCO3, Al2O3, Ga2O3, Sc2O3, In2O3, GeO2 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and reacted at 1200°C for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor NaSr2CGe5O 14 :0.07Cr 3+ (C=Al,Ga,Sc,In) phosphor. Its blue light absorption efficiency, internal and external quantum efficiency and luminescence thermal stability are shown in Table 2. Comparative Example 7-8: NaB2ScGe5O 14 :0.07Cr 3+ ,Yb 3+ Preparation of (B=Ca, Sr) phosphor

[0058] According to the stoichiometric ratio of each element in the chemical formula, high-purity powder raw materials of Na2CO3, CaCO3, SrCO3, Sc2O3, GeO2, Yb2O3 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and reacted at 1200℃ for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor NaCa2ScGe5O 14 :0.07Cr 3+ Phosphor. Its blue light absorption efficiency, internal and external quantum efficiency and luminescence thermal stability are shown in Table 2.

[0059] Comparative Examples 9-10: ASr2ScGe5O 14 :0.07Cr 3+ Preparation of (A=Li,K) phosphor

[0060] According to the stoichiometric ratio of each element in the chemical formula, high-purity powder raw materials of Li2CO3, K2CO3, SrCO3, Sc2O3, GeO2 and Cr2O3 were accurately weighed and placed in an agate mortar for about 30 minutes to fully mix the raw materials. The mixed raw materials were transferred to an alumina crucible and reacted at 1200℃ for 6 hours in an air atmosphere high-temperature reactor. After natural cooling, the near-infrared phosphor ASr2ScGe5O 14 :0.07Cr 3+ (A=Li,K) phosphor. Its blue light absorption efficiency, internal and external quantum efficiency and luminescence thermal stability are shown in Table 2.

[0061] The phases of the samples of the embodiments and comparative examples were analyzed by X-ray powder diffractometer (D8 advanced, Germany).

[0062] The excitation and emission spectra of the samples were measured using an FLS980 (Edinburgh Instruments) fluorescence spectrometer. Combined with a 77–600 K variable temperature stage, the variable temperature emission spectra of the materials were tested to evaluate the thermal stability of the materials.

[0063] A fiber optic spectrometer (ATP5020R) was used to test the luminescence quantum yield of the material through fiber coupling and integrating sphere.

[0064] The samples synthesized by solid phase reaction method show pure phase by XRD analysis. The fluorescent glass ceramics obtained after high temperature melting and crystallization treatment have some impurities, which do not affect their luminescence performance. For example, the XRD diffraction pattern of the near-infrared fluorescent glass ceramics prepared in Example 1 is as follows: Figure 1 shown.

[0065] The excitation and emission spectra of the samples were measured using a FLS980 (Edinburgh Instruments) fluorescence spectrometer. The excitation and emission spectra of the luminescent material of Example 1 are shown in Figure 2 As shown, the excitation spectrum of the luminescent material contains three effective excitation bands, namely 250-350nm, 420-580nm and 600-800nm; it can be seen that the emission spectrum of the luminescent material covers 700-1500nm, that is, it has near-infrared broadband emission performance. Figure 3 The excitation and emission spectra of Example 1 and Comparative Example 1 of the present invention show that the luminescence intensity of the glass ceramic material is significantly stronger than that of the powder material. The absorption efficiency and external quantum efficiency of the examples and comparative examples are shown in Table 1. The blue light absorption efficiency, external quantum efficiency and thermal stability of the glass ceramics with the same chemical structure are better than those of the powder material.

[0066]

[0067] Table 2

[0068]

[0069]

[0070] It should be understood that the above detailed description of the technical solution of the present invention with the help of optimized embodiments is illustrative rather than restrictive, and it cannot be determined that the specific implementation methods of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, modifications to the technical solutions recorded in the embodiments, or equivalent replacement of some of the technical features therein, should be deemed to fall within the scope of patent protection determined by the claims submitted for the present invention.

[0071] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An oxide near-infrared luminescent glass-ceramic material, characterized in that: The chemical formula of the material is A m B n C p D5O 14 :xCr 3+ ,yLn 3+ ; Wherein, A is one or a combination of two or more of the alkali metals Li, Na, K, Rb and Cs; B is one or a combination of two or more of the elements Mg, Ca, Sr, Ba and Zn; C is one or a combination of two or more of Al, Ga, In, Fe, Nb, Ta and rare earth elements; D is one or a combination of two or more of the elements Ti, Si, Ge, Zr, Sn and Hf; Ln is one or more rare earth elements selected from Yb, Nd, Pr, Eu, Dy and Sm; Cr 3+ is the luminescent central ion, Ln 3+ is a sensitizing ion, where 0≤m≤2.5, 1≤n≤4, 0≤p≤1.5, 0% <x≤100%,0%≤y≤20%。 2. The oxide near-infrared luminescent glass-ceramic material according to claim 1, characterized in that: The preparation method comprises the following steps: 1) According to the chemical formula A m B n C p D5O 14 :xCr 3+ ,yLn 3+ Weigh compound raw materials containing each element in a stoichiometric ratio, grind and mix them to obtain a raw material mixture; 2) calcining the mixture obtained in step 1) at high temperature, cooling it to room temperature, and then grinding and sieving it to obtain a powder material; 3) melting the powder material obtained in step 2) at high temperature, cooling and annealing to obtain a glass precursor; 4) The glass precursor obtained in step 3) is crystallized in an air atmosphere by an amorphous crystallization method, and then the crystallized material is post-processed to obtain the oxide near-infrared glass ceramic.

3. The preparation method according to claim 2, characterized in that: In step 1), the grinding time is 5-60 min.

4. The preparation method according to claim 2, characterized in that: In step 2), the high-temperature calcination is carried out in air or an inert atmosphere, the calcination temperature is 1000-1400° C., and the calcination time is 1-24 hours.

5. The preparation method according to claim 2, characterized in that: In step 3), the melting temperature is 1300-1600° C., and the melting time is 0.2-4 h; the annealing temperature is 450-600° C., and the annealing time is 3-10 h.

6. The preparation method according to claim 2, characterized in that: In step 4), the amorphous crystallization method is thermal crystallization, the crystallization temperature is 650-1000°C, and the crystallization time is 1-24h; the post-treatment includes polishing with 180 mesh, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh sandpaper respectively, and then polishing with polishing powder, washing and drying.

Citation Information

Patent Citations

  • Oxide near-infrared light-emitting material, preparation method thereof and light-emitting device

    CN113817468A

  • High-performance oxide near-infrared luminescent material as well as preparation method and application thereof

    CN115322773A

  • Oxide near-infrared light-emitting material, preparation method thereof and light-emitting device

    CN115521785A

  • Oxide near-infrared luminescent glass ceramic and preparation method thereof

    CN116715441A

  • Near-infrared luminescent material, preparation method thereof and LED light source containing near-infrared luminescent material

    CN116751588A

Cited By

  • Novel near-infrared ultrathin fluorescent glass and preparation method thereof

    CN119430664A