Method for regulating and controlling grain growth characteristics of NiZn ferrite film at low temperature
By adding oxidant NaNO2 to the oxidizing solution to control the oxidant concentration, the grain growth characteristics of the NiZn ferrite film are optimized, the problem of insufficient grain growth of the NiZn ferrite film at low temperatures is solved, and high crystallinity and high saturation magnetization are achieved. Thin film preparation, suitable for microwave/millimeter wave monolithic integrated circuits, compatible with semiconductor processes, simplifying the preparation process and saving energy.
Patent Information
- Application Number
- CN202410892525.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
AI Technical Summary
It is difficult to prepare NiZn ferrite thin films with high crystallinity, high saturation magnetization and low coercivity at low temperatures using existing technology. Moreover, it is difficult to control the grain growth characteristics of NiZn thin films prepared by spin spraying and cannot meet the needs of microwave/millimetre-wave monoliths. Low temperature deposition requirements for integrated circuits.
By adding the appropriate oxidant NaNO2 to the oxidation solution, regulating the oxidant concentration, optimizing the grain growth characteristics of the NiZn ferrite film, achieving (222) preferential orientation growth on the non-oriented glass substrate, and improving the saturation magnetization and grain boundaries of the film characteristics, avoid high temperature annealing treatment.
It achieves the preparation of high-crystallinity NiZn ferrite films at low temperatures, with maximum saturation magnetization, significantly enhanced grain orientation, easy operation, compatible with semiconductor processes, energy-saving and efficient, and avoids the deterioration of material properties caused by high-temperature annealing.
Smart Images

Figure CN118851587A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of film preparation, and in particular relates to a method for regulating and controlling the grain growth characteristics of a NiZn ferrite film at low temperature. Background Art
[0002] With the continuous upgrading of communication equipment in recent years, electronic equipment has made extensive use of System on Chip (SOC), Micro System (MS) and System in a Package (SIP), aiming to integrate more functions into a single chip or package to provide more processing power, storage capacity and connection performance to meet the urgent needs of the current whole system for high frequency, small size and light weight, high reliability and multi-function. Inductors have functions such as coupling, energy storage and filtering. They are often used in resonant circuits in combination with capacitors and resistors. They have important application scenarios in consumer electronics, industrial equipment, radio frequency communications and energy transmission. Traditional systems on chip mostly use air-core coil inductors, but their inductance per unit area is low and it is difficult to meet the miniaturization requirements of devices. Thin-film inductors have attracted much attention due to the improvement of thin film preparation technology and the development of semiconductor processes in recent years. Compared with traditional coil inductors, they have smaller size and volume, which makes thin-film inductors easily integrated into micro devices, integrated circuits and other compact electronic products to meet the requirements of modern electronic devices for small size and light weight.
[0003] NiZn ferrite thin films are often used as the preferred material for microwave integrated devices due to their excellent magnetic properties. However, traditional ferrite thin film preparation technologies (sputtering, PLD, thermal decomposition, sol-gel, liquid phase epitaxy, etc.) require high temperatures above 600°C to fully crystallize, which cannot meet the low temperature deposition requirements (<300°C) of magnetic devices such as microwave / millimeter wave monolithic integrated circuits. Therefore, how to prepare high crystallinity and high saturation magnetization 4πM at low temperatures? s and low coercivity H c Making NiZn ferrite film compatible with contemporary semiconductor processes and enabling its application in high-performance thin-film inductors based on system-on-chip is a major issue that needs to be urgently addressed in the rapid development of the electronics industry with SOC-MS-SIP as the core.
[0004] Spin spraying is a technique proposed by Masanori Abe et al. based on the ferrite electroplating wet process (Masanori, Abe, Yutaka, et al. Ferrite-Plating in Aqueous Solution: A New Method for Preparing Magnetic Thin Film [J]. Japanese Journal of Applied Physics, 1983. DOI: 10.1143 / JJAP.22.L511.). By introducing a rotating disk and a droplet nozzle, a crystalline ferrite film is deposited directly in an aqueous solution at a low temperature (<100°C) without any annealing treatment (Abe M, Tamaura Y, Goto Y, et al. High speed deposition of high-quality ferrite films from aqueous solution at low temperatures (≤90°C) [J]. Journal of Applied Physics, 1987, 61 (8): 3211-3213. DOI: 10.1063 / 1.338904.). The highly anticipated low-temperature ferrite preparation technology (spin-spray coating) has been shown to be compatible with substrates such as polymers, glass, printed circuit boards, and radio frequency integrated circuits (Wang X, Chen H, Shi X, et al. A novel NiZn ferrite integrated magnetic solenoid inductor with a highquality factor at 0.7–6GHz[J]. Aip Advances, 2017, 7(5): 056606. DOI: 10.1063 / 1.4973283.), and can directly prepare dense, highly crystalline ferrite films at low temperatures (<90°C). Obi O et al. prepared a 0.7μm thick NiZn ferrite film on a 0.1mm thick glass substrate at low temperature by spin-spray coating. 0.27 Zn 0.1 Fe 2.63 O4 film, the saturation magnetization and in-plane coercivity of the film are 358emu·cm when the external magnetic field is 360Oe. -3and 11Oe, the magnetic permeability of the film increased by 3 times compared with the film grown without magnetic field induction, but the NiZn film prepared under this condition did not show obvious oriented growth (Obi O, Liu M, Lou J, et al. Spin-spray deposited NiZn-Ferrite films exhibiting μr′>50at GHz range[J]. Journal of Applied Physics, 2011, 109(7Pt.3):7127. DOI:10.1063 / 1.3562879.). Wang X et al. prepared Ni on a 0.2 mm thick glass substrate by spin spraying. 0.27 Zn 0.1 Fe 2.63 O4 film, thickness 0.7 μm, preparation temperature 90 °C, deposition rate about 40 nm·min -1 , the grain size of NiZn thin film can be regulated by adjusting the pH value of oxidizing solution and reducing solution, so as to optimize the magnetic properties of thin film. The experiment found that when the pH value of oxidizing solution and reducing solution was adjusted to 9.6 and 4.6 respectively, the grain size of thin film reached the minimum value of 70nm, and the magnetic permeability of thin film was the largest at this time. Especially when the working frequency was 0.5GHz, the initial magnetic permeability of thin film exceeded 200, but no preferential orientation characteristics appeared. Based on the above, the magnetic properties of ferrite thin film can be optimized by adjusting the pH value of reaction solution (Wang X, Zhou Z, Behugn S, et al. Growth behavior and RF / microwave properties of low temperaturespin-sprayed NiZn ferrite[J]. Journal of Materials Science Materials in Electronics, 2015, 26(3): 1890-1894. DOI: 10.1007 / s10854-014-2625-4.).
[0005] The Chinese patent publication number is CN202110225386.6, which discloses a method for preparing a NiZn ferrite film. The NiZn ferrite film is prepared by a rotary spraying method. 0.17 Zn 0.52 Fe 2.31O4 film, by reducing the pH value of the oxidation solution, the film saturation magnetization Ms is increased by nearly 25%, but the experimental operation is relatively complicated. The Chinese patent publication number is CN201910202780.0, which discloses a method for preparing a NiZn ferrite film. First, a thin layer of NiZn ferrite coating is prepared as a seed layer using a rotary spraying technique, and then a ferrite film Ni is deposited on this basis using radio frequency magnetron sputtering. 0.27 Zn 0.03 Fe 2.7 O4, the sputtering temperature needs to be between 100 and 300 °C, where the low-temperature preparation process is only used for the seed layer and there is no regulation on the crystal growth.
[0006] In summary, there is currently no simple and effective technology to control the grain growth characteristics of NiZn ferrite thin films prepared by spin spraying. In addition, regarding the research on grain orientation of ferrite thin films, most of the epitaxial growth of textured thin films is currently achieved by using specific substrates with orientation, and even high-temperature annealing is required to increase the orientation strength, and these complex preparation processes will reduce the performance of the material. Summary of the invention
[0007] The present invention aims to solve the problems of insufficient grain growth power and low saturation magnetization in NiZn ferrite thin films, and proposes a method for regulating the grain growth characteristics of NiZn ferrite thin films at low temperature. The present invention optimizes the grain growth characteristics of NiZn ferrite thin films by adding an appropriate oxidant NaNO2. Without changing the pH value of the solution, the concentration of the main formula and the process parameters of the equipment, the present invention achieves the optimization of grain growth and regulation of grain morphology of NiZn ferrite thin films grown on non-oriented glass substrates by only regulating the concentration of the oxidant in the oxidizing solution. After the regulation, the film sample has obvious triangular grains, indicating that the (222) preferred orientation is enhanced, which can optimize the grain boundary characteristics, and the concentration reaches 3.27mMol·L -1 When (222) is the most oriented film, the saturation magnetization intensity is the largest, and 4πMs is 3908Gs.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A method for regulating the grain growth characteristics of a NiZn ferrite thin film at low temperature comprises the following steps:
[0010] Step 1: Cleaning the reaction table:
[0011] Use 2000-grit sandpaper to polish the reaction table until the surface is smooth and free of foreign matter, wash it with anhydrous ethanol and dry it naturally; select a non-oriented glass substrate with a diameter of Φ12.7mm and a thickness of 0.2mm, clean it ultrasonically, blow it dry with a nitrogen gun and adsorb it on the reaction table;
[0012] Step 2: Solution preparation:
[0013] 2.1 Use NaNO2 as oxidant and CH3COONa as buffer, add deionized water and mix well to obtain oxidant solution; wherein the molar concentration of NaNO2 is 2.18~5.45mmol·L -1 , the molar concentration of CH3COONa is 17.39mmol·L -1 ;
[0014] 2.2 FeCl2, ZnCl2 and NiCl2·6H2O were used as reducing agents, and deionized water was added and mixed to obtain a reducing agent solution; the molar concentration of FeCl2 was 9.09mmol·L -1 , the molar concentration of ZnCl2 is 0.95mmol·L -1 , the molar concentration of NiCl2·6H2O is 1.79mmol·L -1 ;
[0015] Step 3: Parameter setting:
[0016] After starting up, check the operating status of each system, turn on the air compressor and ventilation device, adjust the position of the robot arm, and set the parameters of the spin coating equipment, where the substrate temperature is set to 92°C and the nozzle flow rate is 17ml·min -1 , atomization power 0.3W, working pressure 0.03Mpa, reaction table speed 130rpm;
[0017] Step 4: Film preparation:
[0018] First, the nozzle was connected to deionized water, and the rotation and heating device were turned on to allow the high-speed rotating droplets to form a uniform water film on the surface of the substrate; then when the substrate temperature was stabilized at 92°C, the nozzle was connected to the oxidant solution and the reductant solution respectively, and the reaction was continued for 20 minutes. After the film growth was completed, a NiZn ferrite film with a thickness of 1 μm was obtained.
[0019] According to relevant testing standards, the performance of the obtained NiZn ferrite film was tested using testing equipment such as X-ray diffraction (XRD), vibrating sample magnetometer (VSM), scanning electron microscope (SEM) and vector network analyzer (VNA).
[0020] Furthermore, by adjusting the concentration of the oxidant (2.18-5.45 mmol·L -1 ), realizing the preparation of (222) preferentially oriented NiZn ferrite films.
[0021] In step 2, when preparing the solution, the oxidizing solution is prepared first and the reducing solution is prepared later to prevent the reducing agent solution from being exposed to the air environment for a long time, which may cause Fe 2+ The partial oxidation of
[0022] The present invention provides a method for regulating the grain growth characteristics of NiZn ferrite thin film at low temperature. The core regulation mechanism is that the experimental process is usually carried out in an air environment at normal temperature and pressure. Through the verification of the experiment without adding an oxidant, it is found that the power provided by oxygen in the air is difficult to promote the redox reaction during the film deposition process. The addition of an appropriate oxidant can optimize the grain growth characteristics of the NiZn ferrite thin film. Only the concentration of the oxidant needs to be changed without changing any process parameters to optimize the grain growth and regulate the grain boundary, and produce a triangular morphology (222) preferred orientation. At the same time, the invention does not require high-temperature annealing treatment to obtain a NiZn ferrite thin film with high crystallinity. This low-temperature preparation technology is compatible with semiconductor processes and is easy to operate and controllable.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention provides a method for low-temperature regulation of NiZn ferrite thin film grain growth characteristics. It does not require a substrate with a specific orientation. A non-oriented glass substrate can be used to produce (222) oriented triangular morphology grains. It has a wide range of applications and high application value.
[0025] 2. The present invention provides a method for regulating the grain growth characteristics of NiZn ferrite thin films at low temperature. By properly regulating the concentration of the oxidant, the grain growth characteristics of the NiZn ferrite thin film are optimized, and triangular grains with (222) crystal orientation growth are prepared, and the saturation magnetization intensity is enhanced. Compared with the existing process, the method has simple reaction conditions, controllable operation, energy saving and high efficiency, and a 1μm high-crystalline NiZn ferrite film can be prepared in 20 minutes.
[0026] 3. The present invention provides a method for low-temperature regulation of grain growth characteristics of NiZn ferrite thin films. The NiZn ferrite thin films are prepared by rotary spraying. High-temperature annealing treatment at 600 to 1000°C is not required, which saves energy and preparation time. At the same time, the deterioration of material properties caused by annealing is avoided, and efficient compatibility with semiconductor processes and integrated devices can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 For comparative example (1.09mmol·L -1 )、Example 1(2.18mmol·L -1 )、Example 2 (3.27mmol·L -1 )、Example 3 (4.36mmol·L-1 ) and Example 4 (5.45mmol·L -1 ) obtained NiZn ferrite film XRD pattern;
[0028] Figure 2 The scanning electron microscope photographs of the NiZn ferrite thin films obtained in Comparative Example (a), Example 1 (b), Example 2 (c), Example 3 (d) and Example 4 (e);
[0029] Figure 3 hysteresis loop diagram of the NiZn ferrite film obtained in the comparative example and examples 1 to 4;
[0030] Figure 4 Magnetic spectrum curves of NiZn ferrite films obtained in Comparative Example (a) and Example 2 (b). DETAILED DESCRIPTION
[0031] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0032] Example 1
[0033] A method for low temperature control of NiZn ferrite thin film grain growth characteristics, specifically comprising the following steps:
[0034] Step 1: Cleaning the reaction table:
[0035] Use 2000-grit sandpaper to polish the reaction table until the surface is smooth and free of foreign matter, wash it with anhydrous ethanol and dry it naturally; select a non-oriented glass substrate with a diameter of Φ12.7mm and a thickness of 0.2mm, clean it ultrasonically, blow it dry with a nitrogen gun and adsorb it on the reaction table;
[0036] Step 2: Solution preparation:
[0037] 2.1 With a molar concentration of 2.18 mmol·L -1 NaNO2 is used as an oxidant with a molar concentration of 17.39 mmol·L -1 CH3COONa is used as a buffer, and deionized water is added and mixed evenly to obtain an oxidant solution;
[0038] 2.2 FeCl2, ZnCl2 and NiCl2·6H2O were used as reducing agents, and deionized water was added and mixed to obtain a reducing agent solution; the molar concentration of FeCl2 was 9.09mmol·L -1 , the molar concentration of ZnCl2 is 0.95mmol·L -1 , the molar concentration of NiCl2·6H2O is 1.79mmol·L -1 ;
[0039] Step 3: Parameter setting:
[0040] After starting up, check the operating status of each system, turn on the air compressor and ventilation device, adjust the position of the robot arm, and set the parameters of the spin coating equipment, where the substrate temperature is set to 92°C and the nozzle flow rate is 17ml·min -1 , atomization power 0.3W, working pressure 0.03Mpa, reaction table speed 130rpm;
[0041] Step 4: Film preparation:
[0042] First, the nozzle was connected to deionized water, and the rotation and heating device were turned on to allow the high-speed rotating droplets to form a uniform water film on the substrate surface; then when the substrate temperature was stabilized at 92°C, the nozzle was connected to the oxidant solution and the reductant solution respectively, and the reaction was continued for 20 minutes. After the film growth was completed, a NiZn ferrite film with a thickness of 1 μm was obtained. The entire experiment was carried out in an air environment.
[0043] According to relevant testing standards, the performance of the obtained NiZn ferrite film was tested using testing equipment such as X-ray diffraction (XRD), vibrating sample magnetometer (VSM), scanning electron microscope (SEM) and vector network analyzer (VNA).
[0044] Example 2
[0045] The difference between this embodiment and embodiment 1 is that when preparing the solution in step 2, the molar concentration of the oxidant NaNO2 is adjusted to 3.27 mmol·L -1 , the remaining steps are exactly the same as those in Example 1.
[0046] Example 3
[0047] The difference between this embodiment and embodiment 1 is that when preparing the solution in step 2, the molar concentration of the oxidant NaNO2 is adjusted to 4.36 mmol·L -1 , the remaining steps are exactly the same as those in Example 1.
[0048] Example 4
[0049] The difference between this embodiment and embodiment 1 is that when preparing the solution in step 2, the molar concentration of the oxidant NaNO2 is adjusted to 5.45 mmol·L -1 , the remaining steps are exactly the same as those in Example 1.
[0050] Comparative Example
[0051] The difference between the comparative example and the example 1 is that when preparing the solution in step 2, the molar concentration of the oxidant NaNO2 is adjusted to 1.09 mmol·L -1 , the remaining steps are exactly the same as those in Example 1.
[0052] The test results of the comparative example and embodiments 1 to 4 are shown in the following table:
[0053]
[0054] Figure 1 The XRD spectra of the NiZn ferrite films obtained from the comparative example and Examples 1 to 4 show that the (222) orientation of Examples 1 to 4 is obvious relative to that of the comparative example, that is, the (222) orientation of the NiZn ferrite film is enhanced by increasing the molar concentration of the oxidant NaNO2 in the oxidizing solution.
[0055] Figure 2 The scanning electron microscope photos of the NiZn ferrite films obtained in the comparative example and Examples 1 to 4 show that the grain growth of the NiZn ferrite films in Examples 1 to 3 is effectively improved compared with the comparative example, and obvious grain boundaries appear. Among them, the grain control in Example 2 is the best, and triangular grains appear, indicating that the (222) orientation is enhanced, which is consistent with the XRD characterization results, proving that the grain growth characteristics can be effectively improved by adjusting the oxidant concentration.
[0056] Figure 3 ] are hysteresis loop diagrams of the NiZn ferrite thin films obtained in the comparative example and examples 1 to 4. The results show that the saturation magnetization intensity of examples 1 to 4 is higher than that of the comparative example.
[0057] Figure 4 The magnetic spectrum curves of the NiZn ferrite films obtained in the comparative example and embodiment 2 show that the magnetic permeability is improved.
Claims
1. A method for regulating the grain growth characteristics of NiZn ferrite thin films at low temperature, It is characterized in that The following steps are involved: Step 1: Cleaning the reaction table: Use sandpaper to polish the reaction table until the surface is smooth, clean it with anhydrous ethanol and dry it naturally; select a non-oriented glass substrate, perform ultrasonic cleaning, blow dry it with a nitrogen gun, and then adsorb it on the reaction table; Step 2: Solution preparation: 2.1 with NaNO 2 As an oxidant, CH 3 COONa was used as a buffer, and deionized water was added and mixed evenly to obtain an oxidant solution; among them, NaNO 2 The molar concentration is 2.18~5.45mmol·L -1 , CH 3 The molar concentration of COONa is 17.39 mmol·L -1 ; 2.2 FeCl 2 、ZnCl 2 and NiCl 2 6H 2 O is used as a reducing agent, and deionized water is added and mixed evenly to obtain a reducing agent solution; FeCl 2 The molar concentration is 9.09mmol·L -1 , ZnCl 2 The molar concentration is 0.95mmol·L -1 , NiCl 2 6H 2 The molar concentration of O is 1.79 mmol·L -1 ; Step 3: Parameter setting: Set the parameters of the spin coating equipment, where the substrate temperature is set to 92°C and the nozzle flow rate is 17 ml min -1 , atomization power 0.3W, working pressure 0.03Mpa, reaction table speed 130rpm; Step 4: Film preparation: First, the nozzle was connected to deionized water, and the rotation and heating device were turned on to form a uniform water film on the surface of the substrate; then when the substrate temperature was stabilized at 92°C, the nozzle was connected to the oxidant solution and the reductant solution respectively, and the reaction was continued for 20 minutes. After the film growth was completed, a NiZn ferrite film with a thickness of 1 μm was obtained.
2. The method for controlling the grain growth characteristics of NiZn ferrite thin films at low temperature according to claim 1, It is characterized in that By regulating the concentration of the oxidant, the preparation of NiZn ferrite films with (222) preferential orientation was achieved.
3. The method for controlling the grain growth characteristics of NiZn ferrite thin films at low temperature according to claim 1, It is characterized in that When preparing the solution in step 2, the oxidizing solution is prepared first and the reducing solution is prepared later.