Semi-hydrated phosphogypsum whitening method

By mixing phosphogypsum with a co-solvent and then calcining it under vacuum conditions, the problem of low whiteness and pollution of phosphogypsum in the existing technology is solved, and the whiteness and strength of phosphogypsum are efficiently improved, which is suitable for a variety of application scenarios.

CN118851601APending Publication Date: 2024-10-29GUIZHOU INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410746306.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing phosphogypsum whitening process is time-consuming, consumes a lot of materials, and pollutes serious harmful waste liquids. It is difficult to effectively improve the whiteness and strength of phosphogypsum with existing technology, and there is a lack of efficient cleaning methods suitable for large-scale red mud solid waste treatment.

Method used

Mix phosphogypsum raw residue powder with co-solvent (ammonium bifluoride, barium chloride, ammonium chloride, boric acid) and perform vacuum calcination. Control the temperature at 120~160℃, the vacuum degree at 0.05~0.1MPa, and the calcination time is 2~3 hours, and after cooling, hemihydrate phosphogypsum with higher whiteness is obtained.

Benefits of technology

The whiteness of phosphogypsum has been significantly improved from about 46.7% to more than 90%. The content of hemihydrate phosphogypsum has reached more than 90%. It has short setting and hardening time and high strength. It is suitable for handicrafts, architectural decoration and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851601A_ABST
    Figure CN118851601A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ardealite resource utilization, in particular to a semi-hydrated ardealite whitening method. The invention provides a semi-hydrated ardealite whitening method, which comprises the following steps: uniformly mixing ardealite original slag powder with a cosolvent (ammonium bifluoride, barium chloride, ammonium chloride and boric acid), calcining at 120-160 DEG C, cooling to obtain ardealite with high whiteness, and reacting ions with the cosolvent to avoid generation of other compounds. The whiteness of the phosphogypsum is effectively improved, and meanwhile, the phosphogypsum is dehydrated in the calcining process, so that the whitened semi-hydrated gypsum is obtained. The method is simple and easy to implement, the amount of the needed cosolvent is small, the whiteness effect of the phosphogypsum is remarkable, the whiteness is improved from about 46.7% to 90% or above, and the content of semi-hydrated phosphogypsum is 90% or above. The semi-hydrated phosphogypsum is short in setting and hardening time and relatively high in strength, can be used for handicrafts, architectural costumes, interior and exterior decoration of buildings and the like, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phosphogypsum resource utilization, in particular to a method for whitening semi-hydrated phosphogypsum. Background Art

[0002] Phosphogypsum is a common industrial waste residue in the production process of phosphoric acid. It is a solid waste formed by treating phosphate ore with sulfuric acid. It contains a large amount of insoluble impurities, such as quartz, apatite, insoluble P2O5, eutectic P2O5, fluoride, and soluble impurities such as fluorine, aluminum, magnesium phosphorus, sulfate, and water-soluble P2O5, as well as trace amounts of radioactive elements. The impurities such as fluorine, phosphorus, phosphorus, and phosphorus it contains will cause pollution to the water, atmosphere, and soil environment.

[0003] Most of the existing whitening phosphogypsum processes use flotation, calcination, acid leaching, etc. These processes have problems and defects, such as being time-consuming, high material consumption, and harmful waste liquids that have certain environmental pollution issues.

[0004] For example, patent application CN102923752A discloses a new decolorization and bleaching process for phosphogypsum. The process is cumbersome and time-consuming, and the treatment effect on low-whiteness phosphogypsum is poor in actual production.

[0005] Patent application CN111792663A discloses that bleached continuous gypsum is obtained by calcining phosphogypsum and calcining additives, then preparing the total suspension and reacting it with sulfuric acid, and then filtering and drying. The above two steps are both complicated, time-consuming and labor-intensive, and after adding sulfuric acid, wastewater treatment and other processes are also added.

[0006] Patent application CN109180036A discloses a method of impregnating phosphogypsum with ammonium citrate solution, followed by filtering, washing and drying to obtain decolorized and bleached phosphogypsum. This process requires the addition of ammonium citrate solution, wastewater treatment and other processes, which is cumbersome and time-consuming, and the resulting phosphogypsum has low strength. Therefore, it is an urgent problem to find a new clean and efficient sodium solidification technology suitable for treating large-scale red mud solid waste to improve the conventional red mud de-sodium method.

[0007] Patent CN114477815A discloses a method for rapid whitening of phosphogypsum, which uses high-temperature calcination and ultimately obtains type II anhydrous gypsum. This method involves sulfuric acid, nitric acid and hydrochloric acid. Firstly, improper operation can easily cause chemical reactions with other substances, produce toxic gases, explosions or fires, and increase workplace safety risks. Secondly, leakage or discharge can pollute soil, water and air.

[0008] Therefore, it is currently urgent to find a method that can fully improve the whiteness of phosphogypsum and make full use of phosphogypsum. Summary of the invention

[0009] In order to solve the above technical problems existing in the prior art, the present invention provides a method for whitening hemihydrate phosphogypsum, which is as follows:

[0010] A method for whitening semi-hydrated phosphogypsum comprises the following steps: uniformly mixing phosphogypsum slag powder with a co-solvent, calcining the mixture at 120-160° C., and cooling the mixture to obtain phosphogypsum with a high whiteness. The co-solvent is a mixture of any one or more of ammonium bifluoride, barium chloride, ammonium chloride, and boric acid.

[0011] Furthermore, the calcination parameters are: vacuum degree of 0.05-0.1 MPa, and calcination time of 2-3 hours.

[0012] Furthermore, the mass ratio of the phosphogypsum to the solvent is 1:0.01-0.07.

[0013] Furthermore, the method specifically comprises the following steps:

[0014] (1) Grinding the phosphogypsum residue uniformly;

[0015] (2) adding a solvent to the phosphogypsum and uniformly mixing with the phosphogypsum residue;

[0016] (3) placing the mixed phosphogypsum obtained in step (2) into a vacuum drying oven, and subjecting the mixture to preheating, drying, desorption of attached water, desorption of crystallization water, and calcination, while gradually increasing the temperature to be controlled within the range of 120 to 160° C.;

[0017] (4) Control the temperature within the range of 120 to 160°C, the vacuum degree within the range of 0.05 to 0.1 MPa, and the calcination time within the range of 2 to 3 hours;

[0018] (5) Cooling after calcination is completed.

[0019] Furthermore, the uniform grinding is grinding to 70-300 mesh.

[0020] Furthermore, the cooling is cooling to room temperature.

[0021] Compared with the prior art, the technical effects created by the present invention are embodied in:

[0022] The present application provides a method for whitening semi-hydrated phosphogypsum, wherein the phosphogypsum and a cosolvent are uniformly mixed and then calcined, wherein the ions react with the cosolvent to prevent them from forming other complexes, thereby effectively improving the whiteness of the phosphogypsum. At the same time, the phosphogypsum is dehydrated during the calcination process to obtain whitened semi-hydrated gypsum. The method of the present application is simple and easy to implement, and the amount of cosolvent required is relatively small. The whiteness effect of the phosphogypsum is significant, and the whiteness is increased from about 46.7% to more than 90%, and the content of the semi-hydrated phosphogypsum is more than 90%. The semi-hydrated phosphogypsum obtained has a short setting and hardening time and high strength, and can be used in handicrafts, architectural clothing, and interior and exterior decoration of buildings, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a simplified process flow diagram of this application. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further defined below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.

[0025] Example 1

[0026] ① Take samples of phosphogypsum slag powder and ammonium bifluoride for later use;

[0027] ② Mix phosphogypsum powder and ammonium bifluoride in a mass ratio of 1:0.03, stir and mix evenly for later use;

[0028] ③ Place the spare material in step ② into a vacuum drying oven for calcination, the vacuum degree is 0.05MPa, the calcination temperature is 120°C, and the calcination time is 3h;

[0029] ④ The material calcined in ③ is cooled, and it can be seen that the whiteness is effectively improved to obtain white hemihydrate phosphogypsum. The measured whiteness data is 92.7%, and the hemihydrate phosphogypsum content is 93.5%.

[0030] Example 2

[0031] ① Take samples of phosphogypsum slag powder and barium chloride for later use;

[0032] ② Mix phosphogypsum powder and ammonium bifluoride in a mass ratio of 1:0.05, stir and mix evenly for later use;

[0033] ③ Place the spare material in step ② into a vacuum drying oven for calcination, the vacuum degree is 0.07MPa, the calcination temperature is 140°C, and the calcination time is 2h;

[0034] ④ The material calcined in ③ is cooled, and it can be seen that the whiteness is effectively improved to obtain white hemihydrate phosphogypsum. The measured whiteness data is 93.1%, and the hemihydrate phosphogypsum content is 92.7%.

[0035] Example 3

[0036] ① Take samples of phosphogypsum slag powder and ammonium chloride for later use;

[0037] ② Mix phosphogypsum powder and ammonium bifluoride in a mass ratio of 1:0.07, stir and mix evenly for later use;

[0038] ③ Place the spare material in step ② into a vacuum drying oven for calcination, the vacuum degree is 0.08MPa, the calcination temperature is 120°C, and the calcination time is 3h;

[0039] ④ The material calcined in step ③ is cooled, and it can be seen that the whiteness is effectively improved to obtain white hemihydrate phosphogypsum. The measured whiteness data is 91.5%, and the hemihydrate phosphogypsum content is 93.1%.

[0040] Example 4

[0041] ① Take phosphogypsum slag powder and boric acid samples for later use;

[0042] ② Mix phosphogypsum powder and ammonium bifluoride in a mass ratio of 1:0.06, stir and mix evenly for later use;

[0043] ③ Place the spare material in step ② into a vacuum drying oven for calcination, the vacuum degree is 0.1 MPa, the calcination temperature is 160°C, and the calcination time is h;

[0044] ④ The material calcined in ③ is cooled, and it can be seen that the whiteness is effectively improved to obtain white hemihydrate phosphogypsum. The measured whiteness data is 92.3%, and the hemihydrate phosphogypsum content is 94.1%.

[0045] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the technical solution of the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by ordinary technicians in this field should be considered as the protection scope of the present invention.

Claims

1. A method for whitening hemihydrate phosphogypsum, characterized in that: The raw phosphogypsum slag powder is evenly mixed with a solvent, and then calcined at 120-160° C. After cooling, phosphogypsum with high whiteness is obtained. The solvent is any one or more combinations of ammonium bifluoride, barium chloride, ammonium chloride, and boric acid.

2. The method for whitening hemihydrate phosphogypsum according to claim 1, characterized in that: The calcination parameters are: vacuum degree of 0.05-0.1 MPa, and calcination time of 2-3 hours.

3. The method for whitening hemihydrate phosphogypsum according to claim 1, characterized in that: The mass ratio of the phosphogypsum to the solvent is 1:0.01-0.

07.

4. The method for whitening hemihydrate phosphogypsum according to claim 1, characterized in that: The steps include: (1) Grinding the phosphogypsum residue uniformly; (2) adding a solvent to the phosphogypsum and uniformly mixing with the phosphogypsum residue; (3) placing the mixed phosphogypsum obtained in step (2) into a vacuum drying oven, and subjecting it to preheating, drying, desorption of attached water, desorption of crystallization water, and calcination, with the temperature gradually increased and controlled within a range of 120 to 160° C.; (4) Control the temperature within the range of 120 to 160°C, the vacuum degree within the range of 0.05 to 0.1 MPa, and the calcination time within the range of 2 to 3 hours; (5) Cooling after calcination is completed.

5. The method for whitening hemihydrate phosphogypsum according to claim 4, characterized in that: The uniform grinding is grinding to 70-300 meshes.

6. The method for whitening hemihydrate phosphogypsum according to claim 4, characterized in that: The cooling is cooling to room temperature.