Ultra-high-performance grouting material for prefabricated part splicing and preparation method thereof
Through the combination of specific components and proportions, ultra-high-performance grouting materials without steel fibers are prepared, which solves the problem of difficulty in balancing the fluidity and strength of grouting materials in the existing technology and realizes the splicing and durability of high-performance concrete components. Corrosive, ensuring safe splicing and installation of prefabricated components.
Patent Information
- Application Number
- CN202410869440.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
AI Technical Summary
When existing grouting materials meet the compressive strength and corrosion resistance requirements of high-performance concrete components, it is difficult to balance fluidity and construction convenience. Especially without the use of steel fibers, it is difficult to achieve a 28d compressive strength of more than 140MPa and It has a compressive strength of 56d above 150MPa and excellent anti-corrosion properties.
Using a specific proportion of graded aggregate, nano-silica or nano-calcium carbonate, composite additives and other components, through the close blending of gel materials and admixtures, ultra-high performance grouting materials without steel fibers are prepared, combined with expansion The combination of agent, water retaining agent, viscosity reducer and defoaming agent ensures the high fluidity and strength matching of the grouting material.
It has achieved 28d compressive strength ≥140MPa, 56d compressive strength ≥150MPa, 56d flexural strength ≥34MPa, and has excellent corrosion resistance and construction convenience, ensuring the integrated and safe splicing and installation of prefabricated components.
Smart Images

Figure BDA0004923414930000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement-based grouting materials, and specifically relates to an ultra-high performance grouting material for splicing prefabricated components and a preparation method thereof. Background Art
[0002] In the development process of the infrastructure industry, precast concrete components need to bear increasingly larger loads generated by the operation of equipment, and the requirements for the concrete strength of the components themselves are becoming higher and higher. At present, the compressive strength of ultra-high performance concrete used in large-scale components under construction has reached more than 150MPa, which poses a greater challenge to the grouting materials used for component splicing. As an important material that connects the upper and lower parts of precast component splicing, the performance of grouting materials will directly affect the overall performance of the components after splicing. In addition, the splicing of ultra-high performance concrete precast components requires special material properties and construction technology, and no protective layer is sprayed on the surface after installation. Therefore, in addition to high requirements for fluidity, strength and other properties, the grouting material is required to have the same ultra-high corrosion resistance as the component matrix.
[0003] At present, the research on domestic grouting materials mainly focuses on fluidity (initial and over time) and compressive strength. Some grouting materials on sale have good fluidity but low strength; some grouting materials have good strength but poor fluidity.
[0004] There are also patents involving high-strength grouting materials, such as Chinese patent CN117447131A discloses a fatigue-resistant high-strength wind grouting material and its preparation method and application, which uses cement, mineral admixtures, graded aggregates, water reducers, composite expansion agents, defoamers and nano-hydrated calcium silicate modified fibers. Although it has high fatigue resistance, the compressive strength still cannot reach 150MPa, and it does not involve corrosion resistance. Chinese patent CN115819049A discloses a cement-based grouting material for the installation of a wind power foundation tower base and its preparation method, which is composed of water and a mixture in a mass ratio of 0.08 to 0.09:1, and the mixture includes cement, mineral admixtures, aggregates, composite functional materials and fiber combinations, wherein the fiber combination is composed of steel fibers and polyvinyl alcohol fibers in a mass ratio of 12 to 40:1. Although the fluidity can meet the requirements and the compressive strength reaches 150MPa, the grouting material with added steel fibers cannot be injected and densely spliced gaps when the components are spliced.
[0005] In order to meet the high loads generated by high-power equipment and operation, match the strength performance of ultra-high performance concrete prefabricated components and the corrosion resistance after installation without a protective layer, it is imperative to design an ultra-high performance grouting material that matches the strength of high-performance concrete components, has consistent durability, and is easy to construct and operate, to ensure the integrated and safe splicing and installation of prefabricated components. Summary of the invention
[0006] The technical problem actually solved by the present invention is to provide an ultra-high performance grouting material that can match the strength of high-performance concrete components, has the same durability, and is easy to construct and operate without using steel fibers, thereby ensuring the integrated safe splicing and installation of prefabricated components. The grouting material has a 28d compressive strength of more than 140MPa and a 56d compressive strength of more than 150MPa, and is also an ultra-high performance grouting material with excellent corrosion resistance.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A grouting material for prefabricated component splicing includes a premix, wherein the raw material formula of the premix includes, by weight: 25-35 parts of cement, 1-5 parts of fly ash, 3-10 parts of microspheres, 3-10 parts of silica fume, 1-4 parts of nanomaterials, 45-60 parts of aggregates, 1-4 parts of water reducing agents and 0.5-3 parts of composite additives, wherein:
[0009] Among the aggregates, the aggregates with a particle size of 2.36mm-1.18mm account for 15-25%, the aggregates with a particle size of 1.18mm-0.6mm account for 25-35%, the aggregates with a particle size of 0.6mm-0.3mm account for 25-35%, the aggregates with a particle size of 0.3mm-0.15mm account for 5-15%, and the aggregates with a particle size of less than 0.15mm account for 5-15%;
[0010] The composite additive is a combination of a swelling agent, a water retaining agent, a viscosity reducing agent and a defoaming agent.
[0011] According to some embodiments of the present invention, the raw material formula of the premix includes: 25-32 parts of cement, 2.5-5 parts of fly ash, 3.5-8 parts of microspheres, 4-8 parts of silica fume, 1-4 parts of nanomaterials, 45-60 parts of aggregate, 1-2 parts of water reducer and 0.5-2 parts of composite additives.
[0012] In some specific embodiments, the nanomaterial is at least one of nano silicon dioxide and nano calcium carbonate; wherein the average particle size of nano silicon dioxide is ≤20nm and the purity is ≥99%; the particle size of nano calcium carbonate is 40-80nm and the purity is ≥95%.
[0013] In some specific embodiments, the aggregate is at least one of quartz sand or machine-made sand, has a fineness modulus of 2.6-3.0, and a crushing index of ≤15%.
[0014] In some specific embodiments, in the composite additive, the expander accounts for 82-96%, the water retainer accounts for 0.5-6%, the viscosity reducer accounts for 3-10%, the defoamer accounts for 0-4%, and the defoamer is not zero.
[0015] Furthermore, the expansion agent is a combination of an ettringite expansion agent and a plastic expansion agent. Preferably, the ettringite expansion agent and the plastic expansion agent are combined in a mass ratio of 20:5-10.
[0016] Furthermore, the water retaining agent is cellulose ether, such as cellulose ether with a viscosity of 400.
[0017] Furthermore, the viscosity reducing agent is at least one of sodium gluconate and sodium citrate.
[0018] In some specific embodiments, the grouting material further comprises water, and the amount of the water is 8-9% of the total weight of the premix.
[0019] In some specific embodiments, the cement is ordinary Portland cement, and the ordinary Portland cement is P·I 52.5 Portland cement and / or P·II 52.5 ordinary Portland cement.
[0020] In some specific embodiments, the fly ash is Class I fly ash, with a water demand ratio of ≤95% and an activity index of ≥90%.
[0021] In some specific embodiments, the average particle size of the microbeads is ≤10 μm, the water demand ratio is ≤110%, and the 28d activity index is ≥110%.
[0022] In some specific embodiments, the silica fume is of S95 grade, has a water requirement ratio of ≤120%, and an activity index of ≥110%.
[0023] The second technical solution adopted by the present invention is: a method for preparing the grouting material for splicing prefabricated components as described above, mixing all raw materials of the premix, adding water, and stirring to obtain the grouting material for splicing prefabricated components.
[0024] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0025] The present invention does not use steel fibers, but is based on a specific proportion of graded aggregates, combined with nano-silicon dioxide and the coordination between other components and proportions. The grouting material prepared under conditions of lower water consumption can match the strength of high-performance concrete components, meet the durability requirements, and is convenient to construct and operate. It is used for splicing prefabricated components and can ensure the integrated and safe splicing and installation of prefabricated components. DETAILED DESCRIPTION
[0026] The present invention aims to provide an ultra-high performance grouting material for prefabricated component splicing that can match the strength of high-performance concrete components, is consistent with durability, and is convenient for construction and operation, so as to ensure the integrated safe splicing and installation of prefabricated components. To achieve the above purpose, the present invention is based on the porosity of graded aggregates, through the close matching design of gel materials and admixtures, combined with the use of nanomaterials, and the synergistic effect of various components and proportions, to prepare a grouting material, which achieves significant improvement in mechanical properties and durability on the basis of convenient construction. Without using steel fibers, the grouting material has a water-to-material ratio of 8 to 9%, and obtains a 28d compressive strength ≥140MPa, a 56d compressive strength ≥150MPa, a 56d flexural strength ≥34MPa, a 56d chloride ion penetration resistance (coulometric method) ≤100C, and a 56d chloride ion diffusion coefficient ≤1.4×10 -13 m 2 / s ultra-high performance, and the initial fluidity of the grouting material is ≥300mm, and the fluidity after 30min is ≥275mm.
[0027] In addition, although the compressive strength of existing grouting materials can reach 140MPa by adding steel fibers, the steel fiber grouting materials cannot be poured or squeezed into the joints of prefabricated components during construction. However, the grouting material of this application does not add steel fibers. By closely stacking the gel material and the aggregate, an ultra-high performance grouting material for splicing ultra-high performance concrete components with a matching strength grade of 150MPa is prepared. The grouting material and ultra-high performance concrete prefabricated components show excellent matching in terms of material composition, mechanical properties, durability and construction technology. This matching enables the two to jointly form an ultra-high performance structural system, providing reliable technical support and quality assurance for modern construction projects.
[0028] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention, but the present invention is not limited to the scope of the examples.
[0029] Example 1
[0030] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is composed of water and premix in a mass ratio of 0.0875:1. The composition of the premix is shown in Table 1.
[0031] Among them, the cement used is P·I 52.5 silicate cement.
[0032] The aggregate is quartz sand with a fineness modulus of 2.6-3.0 and a crushing index of ≤15%. Among them, the particle size of 2.36mm-1.18mm accounts for 19.8%, the particle size of 1.18mm-0.6mm accounts for 29.0%, the particle size of 0.6mm-0.3mm accounts for 28.4%, the particle size of 0.3mm-0.15mm accounts for 11.4%, and the particle size less than 0.15mm accounts for 11.4%.
[0033] The fly ash is Class I fly ash, with a water demand ratio of ≤95% and an activity index of ≥90%.
[0034] The average particle size of the microbeads is ≤10μm, the water demand ratio is ≤110%, and the 28d activity index is ≥110%.
[0035] The silica fume is of S95 grade, with water requirement ratio ≤120% and activity index ≥110%.
[0036] The nano material is nano silicon dioxide, with an average particle size of ≤20nm and a purity of ≥99%.
[0037] The composite additive is composed of an expander, a water retainer, a viscosity reducer and a defoamer, wherein the expander accounts for 92%, the water retainer accounts for 1%, the viscosity reducer accounts for 5% and the defoamer accounts for 2%. Among them, the expander is a combination of an ettringite expander and a plastic expander in a mass ratio of 19:6; the viscosity reducer is sodium citrate.
[0038] The ultra-high performance grouting material is prepared by the following method:
[0039] Pour the premix into a mixer, dry-mix for 1 minute, then add water and mix for 4 minutes to obtain the grouting material.
[0040] Example 2
[0041] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is different from that in Embodiment 1 in that the aggregate is made of pebble-made sand, and the composition of the premix is shown in Table 2.
[0042] Example 3
[0043] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is different from that in Embodiment 1 in that the nano material is 50 nm nano calcium carbonate, and the composition of the premix is shown in Table 2.
[0044] Example 4
[0045] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is different from that in Embodiment 1 in that the nano material is nano silicon dioxide and 50 nm nano calcium carbonate uniformly mixed in a mass ratio of 1:1, and the composition of the premix is shown in Table 2.
[0046] Example 5
[0047] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is different from that in Embodiment 1 in that:
[0048] The composite additive is composed of an expander, a water retainer, a viscosity reducer and a defoamer, wherein the expander accounts for 89%, the water retainer accounts for 1%, the viscosity reducer accounts for 8% and the defoamer accounts for 2%. Among them, the expander is a combination of an ettringite-based expander and a plastic expander in a mass ratio of 19:6, and the viscosity reducer is sodium citrate.
[0049] Example 6
[0050] The ultra-high performance grouting material for prefabricated component splicing provided in this embodiment is different from that in Embodiment 5 in that:
[0051] The viscosity reducer is sodium gluconate.
[0052] Table 1 Components of the premix of ultra-high performance grouting material of Examples 1 to 6 (by weight)
[0053] serial number cement Silica Fume Microbeads Fly ash Nanomaterials aggregate Water reducing agent Compound Additives Example 1 28.4 6.1 7.0 2.2 2.2 51.5 1.3 1.3 Example 2 27.1 6.8 7.0 2.6 2.4 51.3 1.5 1.3 Example 3 29.3 6.1 4.4 4.2 1.9 51.3 1.2 1.3 Example 4 30.5 4.4 4.4 3.3 3.3 51.1 1.7 1.3 Example 5 28.4 6.1 7.0 2.2 2.2 51.5 1.3 1.3 Example 6 28.4 6.1 7.0 2.2 2.2 51.5 1.3 1.3
[0054] Comparative Example 1
[0055] The grouting material provided in this comparative example is different from that in Example 1 in that the aggregate is quartz sand, which is composed of four types of quartz sand particle sizes, of which 8.5% are 2.36mm-1.15mm, 15.4% are 1.15mm-0.6mm, 37.6% are 0.6mm-0.3mm, 25.8% are 0.3mm-0.15mm, and 12.7% are less than 0.15mm.
[0056] Comparative Example 2
[0057] The grouting material provided in this comparative example is different from that in Example 1 in that the aggregate is machine-made sand, which is composed of quartz sand of four particle sizes, of which the particle size of 2.36mm-1.15mm accounts for 8.5%, 1.15mm-0.6mm accounts for 15.4%, 0.6mm-0.3mm accounts for 37.6%, 0.3mm-0.15mm accounts for 25.8%, and the particle size less than 0.15mm accounts for 12.7%.
[0058] Comparative Example 3
[0059] The grouting material provided in this comparative example is different from that in Example 1 in that no nanomaterial is used.
[0060] Comparative Example 4
[0061] The grouting material provided in this comparative example is different from that in Example 1 in that the composite additive is composed of an expansion agent, a water retaining agent and a defoaming agent, wherein the expansion agent accounts for 97%, the water retaining agent accounts for 1% and the defoaming agent accounts for 2%. The expansion agent is a combination of an ettringite expansion agent and a plastic expansion agent in a mass ratio of 19:6.
[0062] Comparative Example 5
[0063] The grouting material provided in this comparative example is different from that in Example 1 in that the composite additive is composed of an expansion agent, a water retaining agent, a viscosity reducing agent and a defoaming agent, wherein the expansion agent accounts for 77%, the water retaining agent accounts for 1%, the viscosity reducing agent accounts for 20% and the defoaming agent accounts for 2%. The expansion agent is a combination of an ettringite expansion agent and a plastic expansion agent in a mass ratio of 19:6, and the viscosity reducing agent is sodium citrate.
[0064] The grouting materials of Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to performance testing with reference to JG / T 408-2019, and the results are shown in Table 2.
[0065] Table 2 Performance test results of grouting materials of Examples 1 to 6 and Comparative Examples 1 to 5
[0066]
[0067] It can be seen from the results in Table 2 that the ultra-high performance grouting material of the representative embodiment of the present invention has good workability (initial ≥300mm, 30min ≥260mm), the final compressive strength of 56d is above 150MPa and the corrosion resistance is excellent. It can be seen from Comparative Examples 1 and 2 that based on the different matching ratios of quartz sand and machine-made sand particle sizes, the final workability and strength results of the grouting material have obvious differences. Well-graded aggregates can make the grouting material more workable and more compact as a whole. The compactness of the high and low strength reaction also affects the durability of the grouting material to a certain extent. It can be seen from Comparative Example 3 that after removing the nanomaterial, the loss of the active reaction and filling effect of the nanomaterial causes the mechanical properties of the grouting material to decline significantly, which is only about 130MPa. Comparative Example 4 shows that the overall viscosity of the grouting material without adding a viscosity reducer is too high. Due to the reduction in flowability, small bubbles are wrapped in during mixing and forming, resulting in initial and 30-minute fluidity of only 281 mm and 254 mm, respectively. Such poor workability makes it difficult for the slurry to compact the vertical and horizontal joints during the prefabricated component splicing construction process. Comparative Example 5 shows that in the composite additive, the viscosity reducer accounts for 20%, and the grouting material has very good workability. However, the excessive dosage seriously affects the slow coagulation and hardening of the grouting material, which significantly reduces the compressive strength and flexural strength and affects the durability.
[0068] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0069] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A grouting material for splicing prefabricated components, comprising a premix, characterized in that: The raw material formula of the premix includes, by weight: 25-35 parts of cement, 1-5 parts of fly ash, 3-10 parts of microspheres, 3-10 parts of silica fume, 1-4 parts of nanomaterials, 45-60 parts of aggregates, 1-4 parts of water reducers and 0.5-3 parts of composite additives, wherein: Among the aggregates, the aggregates with a particle size of 2.36mm-1.18mm account for 15-25%, the aggregates with a particle size of 1.18mm-0.6mm account for 25-35%, the aggregates with a particle size of 0.6mm-0.3mm account for 25-35%, the aggregates with a particle size of 0.3mm-0.15mm account for 5-15%, and the aggregates with a particle size of less than 0.15mm account for 5-15%; The composite additive is a combination of a swelling agent, a water retaining agent, a viscosity reducing agent and a defoaming agent.
2. The grouting material according to claim 1, characterized in that: The raw material formula of the premix includes: 25-32 parts of cement, 2.5-5 parts of fly ash, 3.5-8 parts of microspheres, 4-8 parts of silica fume, 1-4 parts of nano material, 45-60 parts of aggregate, 1-2 parts of water reducing agent and 0.5-2 parts of composite additives.
3. The grouting material according to claim 1 or 2, characterized in that: The nano material is at least one of nano silicon dioxide and nano calcium carbonate; wherein the average particle size of nano silicon dioxide is less than or equal to 20 nm; and the particle size of nano calcium carbonate is 40-80 nm.
4. The grouting material according to claim 1 or 2, characterized in that: The aggregate is at least one of quartz sand or machine-made sand, with a fineness modulus of 2.6-3.0 and a crushing index of ≤15%.
5. The grouting material according to claim 1 or 2, characterized in that: In the composite additive, the expander accounts for 82-96%, the water retainer accounts for 0.5-6%, the viscosity reducer accounts for 3-10%, the defoamer accounts for 0-4%, and the defoamer is not zero.
6. The grouting material according to claim 5, characterized in that: The expansion agent is a combination of an ettringite expansion agent and a plastic expansion agent in a mass ratio of 20:5-10; and / or the water retaining agent is cellulose ether; and / or the viscosity reducing agent is at least one of sodium gluconate and sodium citrate.
7. The grouting material according to claim 1 or 2, characterized in that: The grouting material also includes water, and the amount of the water is 8-9% of the total weight of the premix.
8. The grouting material according to claim 1 or 2, characterized in that: The cement is ordinary Portland cement.
9. The grouting material according to claim 1 or 2, characterized in that: The fly ash is Class I fly ash; and / or the average particle size of the microbeads is ≤10 μm; and / or the silica ash is Class S95.
10. A method for preparing a grouting material for splicing prefabricated components according to any one of claims 1 to 9, characterized in that: All raw materials of the premix are mixed, water is added, and stirred to obtain a grouting material for splicing prefabricated components.