Ultra-light foaming concrete and preparation method thereof

By using trimesoyl chloride and diamine to generate organic additives in concrete, and combining them with modified animal protein foaming agents and ultrafine powders to build a highly cross-linked structure, it solves the problem of lightweight and high-performance foamed concrete. The issue of balance between strength achieves ultra-lightweight foam concrete with high compressive strength and corrosion resistance, meeting the requirements of building materials.

CN118851701APending Publication Date: 2024-10-29ANHUI DONGCAI MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410941550.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing foamed concrete is difficult to balance between the pursuit of lightweight and high strength, resulting in reduced mechanical strength and inability to meet the requirements for high strength and corrosion resistance of building materials.

Method used

By introducing trimesoyl chloride and diamine into concrete for acylation reaction to generate organic additives, combined with modified animal protein foaming agent and ultrafine powder, a network structure with high cross-linking degree is constructed to optimize the internal pores of concrete. Structural and interface bonding, improving compressive strength and corrosion resistance.

Benefits of technology

Ultra-lightweight foamed concrete with low bulk density, high compressive strength and corrosion resistance has been realized, which meets the requirements of building materials and has extremely high practical value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure HDA0004944295070000011
    Figure HDA0004944295070000011
Patent Text Reader

Abstract

The invention relates to the field of building materials (IPC classification number: C04B), in particular to ultra-light foaming concrete and a preparation method thereof. The concrete is prepared from the following raw materials in parts by weight: 250-500 parts of cement, 130-250 parts of superfine powder, 10-70 parts of an organic auxiliary agent, 6-27 parts of a modified animal protein foaming agent and 190-380 parts of water, and reaction raw materials of the organic auxiliary agent comprise trimesoyl chloride and diamine. By introducing the superfine powder, the organic auxiliary agent and the modified animal protein foaming agent, the light, high-strength and corrosion-resistant foamed concrete is obtained, the technical problem that the light weight and high strength of the foamed concrete in the prior art are difficult to balance is solved, the requirements of building materials can be met, and the practical value is extremely high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building materials (IPC classification number: C04B), and in particular to ultra-lightweight foaming concrete and a preparation method thereof. Background Art

[0002] Applying bulk solid waste to building materials to prepare lightweight, high-strength concrete products with closed pores is an innovative move towards sustainable development.

[0003] At present, researchers at home and abroad have tried to introduce organic matter into the inorganic system of concrete, and combine physical / chemical foaming methods to prepare densely porous, high-strength concrete products. Chinese patent CN107572936B prepared a polymer foam concrete, introduced organic binders, organic water-soluble solutions and other components into the concrete formula, and obtained a lightweight, water-resistant and durable polymer foam concrete. Chinese patent CN111747691B prepared a highly crack-resistant foam concrete, and introduced absorbent resins, plant fibers and other components to improve the strength and shrinkage crack resistance of concrete into the formula, and obtained a foam concrete that is anti-shrinkage, anti-cracking and has improved toughness.

[0004] At present, the research and development of foamed concrete mainly focuses on the product characteristics of low bulk density and high mechanical strength. However, a decrease in bulk density usually also leads to a decrease in mechanical strength, and building materials have high requirements for mechanical strength. Therefore, there is an urgent need to provide a foamed concrete product with good comprehensive performance that meets the requirements of lightweight, high strength and corrosion resistance. Summary of the invention

[0005] The present invention solves the technical problem of the difficulty in balancing the lightness and high strength of foamed concrete in the prior art by providing an ultra-lightweight foamed concrete, thereby realizing a foamed concrete with low bulk density, high compressive strength and strong corrosion resistance, which can meet the requirements of building materials and has extremely high practical value.

[0006] The invention provides an ultra-lightweight foaming concrete. The concrete is prepared from raw materials comprising, by weight, 250-500 parts of cement, 130-250 parts of ultrafine powder, 10-70 parts of organic additives, 6-27 parts of foam and 190-380 parts of water.

[0007] Preferably, in parts by weight, the raw materials for preparing the concrete include: 250-500 parts of cement, 130-250 parts of ultrafine powder, 25-50 parts of organic additives, 10-22 parts of foam, and 190-380 parts of water.

[0008] In some preferred embodiments, the organic auxiliary agent includes trimesoyl chloride and diamine.

[0009] Preferably, the diamine is a C3-C15 diamine.

[0010] Preferably, the diamine is a C6-C10 diamine.

[0011] In some preferred embodiments, the diamine is selected from at least one of 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine.

[0012] In some preferred embodiments, the molar ratio of trimesoyl chloride to diamine is 1:(1-5).

[0013] Preferably, the molar ratio of trimesoyl chloride to diamine is 1:(2-4).

[0014] The present invention introduces an organic additive into a concrete system, that is, trimesoyl chloride and a diamine are selected to undergo an acylation reaction, and in particular, trimesoyl chloride and a diamine are selected as reaction raw materials. During the preparation of concrete, a three-dimensional network with an interwoven structure is generated by the reaction. The organic additive can provide a good skeleton structure for the concrete system.

[0015] In some preferred embodiments, the reaction raw materials of the organic auxiliary agent also include an acid binding agent.

[0016] Preferably, the acid binding agent includes at least one of calcium hydroxide, triethylamine, sodium carbonate, potassium carbonate, sodium acetate and sodium bicarbonate.

[0017] Further preferably, the acid binding agent is sodium bicarbonate.

[0018] In some preferred embodiments, the foam is prepared by foaming a modified animal protein foaming agent with water; the raw materials for preparing the modified animal protein foaming agent include animal protein, unsaturated acid chloride and water.

[0019] In some preferred embodiments, the mass ratio of the animal protein, unsaturated acid chloride and water is 1:(0.05-0.5):(1-10).

[0020] Preferably, the mass ratio of the animal protein, unsaturated acyl chloride and water is 1:(0.1-0.2):(2-5).

[0021] In some preferred embodiments, the animal protein is obtained by hydrolyzing and drying waste animal (cow, sheep, horse, donkey, pig, etc.) keratin or animal hair waste as raw materials.

[0022] In some preferred embodiments, the unsaturated acid chloride is an unsaturated aliphatic acid chloride.

[0023] Preferably, the unsaturated acid chloride is an unsaturated aliphatic acid chloride with a terminal olefin.

[0024] More preferably, the unsaturated acid chloride is 10-undecenoyl chloride.

[0025] In some preferred embodiments, the preparation steps of the modified animal protein foaming agent include: mixing animal protein, unsaturated acid chloride and water, stirring at 40-80°C for 2-5 hours, adjusting the pH value of the mixture with hydrochloric acid until precipitation occurs, centrifuging, washing and drying to obtain the modified animal protein foaming agent.

[0026] When using, add the modified animal protein foaming agent and water into the foaming machine to generate foam and set aside.

[0027] The present invention selects unsaturated acyl chloride to improve animal protein and creatively uses it in the field of building materials, which helps to reduce the bulk density of building materials and improve the strength and corrosion resistance of the products. The reasons may be:

[0028] The hydrophobic long-chain olefins in the unsaturated acyl chloride are grafted onto the protein molecules, effectively increasing their surface activity and improving the foaming effect. The double bonds on the unsaturated acyl chloride can bond with the amino groups in the organic additives, working together from two dimensions. On the one hand, the foaming multiple of the foaming agent is increased. On the other hand, the modified animal protein foaming agent cooperates with the organic additives to build a highly cross-linked network structure in the system. The double bonds on the unsaturated acyl chloride are grafted onto the network to make the bubbles in the system arranged regularly and tightly, and improve the stability of the foam. The joint use of modified animal protein foaming agents and organic additives effectively optimizes the internal pore structure of concrete, thereby reducing the bulk density of concrete products while improving the compressive strength and corrosion resistance of concrete products.

[0029] In some preferred embodiments, the mass ratio of the organic additive to the foam is 1:(0.2-0.6). The inventors have found that when the mass ratio of the organic additive to the foam satisfies the above relationship, they can work together in the concrete system to form a highly cross-linked network structure, thereby improving the internal pore structure of the concrete and improving the mechanical strength and corrosion resistance of the product.

[0030] The present invention also introduces superfine powder into the concrete system, and the superfine powder includes at least one of fly ash, slag powder, desulfurized gypsum, silica fume, quicklime, carbide slag and fly ash.

[0031] Preferably, the ultrafine powder includes fly ash, slag powder, desulfurized gypsum, silica fume and quicklime.

[0032] Further preferably, the superfine powder includes 80-160 parts by weight of fly ash, 40-80 parts by weight of slag powder, 20-40 parts by weight of desulfurized gypsum, 8-20 parts by weight of silica fume and 8-20 parts by weight of quicklime. The present invention finds that by using the above-mentioned superfine powder compound, the hydroxyl groups on its surface interact with the active groups such as carboxyl groups on the surface of the modified animal protein foaming agent in the system, effectively improving the organic-inorganic interface bonding force and improving the interface bearing capacity, thereby obtaining a lightweight and durable foamed concrete.

[0033] In some preferred embodiments, the average particle size of the fly ash particles is 1-25 μm; preferably, the average particle size of the fly ash particles is 3-12 μm.

[0034] In some preferred embodiments, the average particle size of the slag powder is 2-30 μm; preferably, the average particle size of the slag powder is 4-15 μm.

[0035] In some preferred embodiments, the specific surface area of ​​the silica fume is 16000-32000m 2 / kg.

[0036] In some preferred embodiments, the average particle size of the quicklime particles is 10-30 μm; preferably, the average particle size of the quicklime particles is 12-16 μm.

[0037] The present invention simultaneously introduces the foam and superfine powder prepared by organic additives and modified animal protein foaming agents in the concrete system, which significantly improves the mechanical properties and corrosion resistance of foamed concrete. Based on this, the inventor speculates that the reason why the concrete performance is optimized is that: on the one hand, after the modified animal protein foaming agent is added to the system, a hydrophobic olefin chain grafted on the protein molecule is introduced, and its terminal olefin is bonded with the amino group in the organic additive, and a network structure with a high degree of crosslinking is woven together, which not only promotes the regular and tight arrangement of bubbles in the system, and the high foam stability, the regular and tight pore structure inside the concrete, not only improves the strength, but also can resist the erosion of external acid radicals to a certain extent. On the other hand, in the reaction process, sodium bicarbonate is used as an acid binding agent, and carbon dioxide can be additionally released, and the physical foaming mode of the coordinated modified animal protein foaming agent is jointly promoted to produce rich and dense bubbles in the system, and the internal pore structure of the foamed concrete with uniform distribution, moderate pore size and orderly arrangement is constructed, and the bulk density of the foamed concrete is effectively reduced. In addition, with the addition of ultrafine powder, the hydroxyl groups on its surface interact with the active groups such as carboxyl groups on the surface of the modified animal protein foaming agent in the system. The product can effectively reduce harmful pores in the system, improve the organic-inorganic interface bonding force, and increase the interface bearing capacity and system density, thereby obtaining a lightweight, high-strength and durable foamed concrete product.

[0038] In some preferred embodiments, the water-cement ratio in the concrete is (0.3-0.7):1, preferably (0.4-0.6):1; that is, the addition amount of cement, ultrafine powder and water satisfies m 水 / m (水泥+超微粉) =(0.4-0.6):1.

[0039] The present invention also provides a method for preparing ultra-lightweight foamed concrete, the preparation steps of the concrete comprising:

[0040] 1) Adding modified animal protein foaming agent and water into a foaming machine to generate foam for standby use;

[0041] 2) Mix cement and ultrafine powder evenly, then add water, stir for 1-20 minutes, then add organic additives, stir for 0.5-5 minutes, then add the foam obtained in step 1) while stirring, stir for 10-60 seconds, pour the material into a mold, let it stand for 1-5 days, then demould, perform standard curing after demoulding, and obtain ultra-lightweight foamed concrete.

[0042] The standard curing conditions are conventional operating methods in the art and are not particularly limited; for example: standard curing for 28 days, during which the temperature is maintained at 20±2° C. and the humidity is not less than 95%.

[0043] Beneficial effects:

[0044] (1) The present invention uses cement, ultrafine powder, organic additives, foam, and water as raw materials to prepare lightweight, high-strength, corrosion-resistant lightweight foamed concrete; the organic additives include trimesoyl chloride and diamine, which can construct a three-dimensional network in the system and form a network structure with an interwoven structure in the concrete system, which has a regular and stabilizing effect on the bubbles in the system, thereby reducing the bulk density of the product and optimizing the mechanical strength of the product.

[0045] (2) The reaction raw materials of the organic additive also include an acid binder, preferably sodium bicarbonate. During the reaction, sodium bicarbonate can release additional CO2 while acting as an acid binder, providing another bubble source for the system, thereby jointly optimizing the internal pore structure of the concrete and improving the performance of the foamed concrete.

[0046] (3) The present invention preferably uses unsaturated acyl chlorides (especially unsaturated aliphatic acyl chlorides with terminal olefins) to modify animal proteins, which can not only increase the foaming multiple of the foaming agent, but also further bond with organic additives to construct a highly cross-linked network structure, thereby reducing the bulk density of the product and improving the mechanical properties of the product.

[0047] (4) The present invention explores the raw material ratio of organic additives and modified animal protein foaming agents to maximize the regular and tight arrangement of bubbles in the system, thereby constructing an internal pore structure with uniform pore distribution, moderate and uniform pore size, and orderly arrangement, thereby improving the mechanical properties while reducing the bulk density of the foamed concrete.

[0048] (5) The present invention adopts fly ash, slag powder, desulfurized gypsum, silica fume and quicklime to obtain ultrafine powder. The hydroxyl groups on the surface of the ultrafine powder interact with the active groups such as carboxyl groups on the surface of the modified animal protein foaming agent in the system. The product can fill the pores, effectively improve the density of the concrete system and the organic-inorganic interface bonding force, and cooperate with organic additives and animal protein foaming agents to obtain a lightweight, high-strength and durable foamed concrete product with extremely high practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a physical picture of the concrete slurry prepared in Example 1;

[0050] Figure 2 This is a physical picture of the concrete prepared in Example 1 being poured into a mold for forming. DETAILED DESCRIPTION

[0051] Example 1

[0052] This embodiment provides an ultra-lightweight foamed concrete. The raw materials for preparing the concrete include, by weight: 350 parts by weight of cement, 180 parts by weight of ultrafine powder, 35 parts by weight of organic additives, 15 parts by weight of foam, and 265 parts by weight of water.

[0053] In parts by weight, the organic auxiliary agent includes 9 parts by weight of trimesoyl chloride, 16 parts by weight of 1,9-nonanediamine and 10 parts by weight of sodium bicarbonate;

[0054] In parts by weight, the raw materials for preparing the modified animal protein foaming agent include 20 parts by weight of animal protein, 3 parts by weight of 10-undecenoyl chloride and 80 parts by weight of water.

[0055] The animal protein is obtained by hydrolyzing and drying bovine keratin as a raw material.

[0056] The modified animal protein foaming agent preparation method comprises: placing animal protein and 10-undecenoyl chloride in water, stirring at 60° C. for 3 hours, adjusting the pH value thereof with hydrochloric acid until precipitation is generated, and then centrifuging and washing to obtain the modified animal protein foaming agent.

[0057] In parts by weight, the ultrafine powder includes 100 parts by weight of fly ash, 50 parts by weight of slag powder, 24 parts by weight of desulfurized gypsum, 10 parts by weight of silica fume and 10 parts by weight of quicklime. 180 parts are added to the concrete.

[0058] The average particle size of the fly ash is 8 μm.

[0059] The average particle size of the slag powder is 10 μm.

[0060] The specific surface area of ​​the silica fume is 20000m 2 / kg.

[0061] The average particle size of the quicklime particles is 14 μm.

[0062] The steps of preparing the concrete include:

[0063] 1) Add the modified animal protein foaming agent into a foaming machine, add 600 parts by weight of water, generate foam, and set aside;

[0064] 2) Mix cement and ultrafine powder evenly, then add water and stir for 5 minutes, then add organic additives and stir for 1.5 minutes, then add the foam obtained in step 1) while stirring, stir for 30 seconds to obtain concrete slurry (see Figure 1 ), introduce the concrete slurry into the mold and let it stand for 1 day (see Figure 2 ), standard curing is carried out after demoulding to obtain ultra-lightweight foamed concrete.

[0065] The standard curing is specifically as follows: standard curing for 28 days, during which the temperature is maintained at 20° C. and the humidity is 98%.

[0066] Example 2

[0067] This embodiment provides an ultra-lightweight foamed concrete. The raw materials for preparing the concrete include, by weight: 250 parts by weight of cement, 130 parts by weight of ultrafine powder, 130 parts by weight of organic additives, 11 parts by weight of foam, and 190 parts by weight of water.

[0068] In parts by weight, the organic auxiliary agent includes 8 parts by weight of trimesoyl chloride, 8.5 parts by weight of 1,7-heptanediamine and 8.5 parts by weight of sodium bicarbonate.

[0069] In parts by weight, the raw materials for preparing the modified animal protein foaming agent include 7 parts by weight of animal protein, 1 part by weight of 10-undecenoyl chloride and 25 parts by weight of water.

[0070] The animal protein is obtained by hydrolyzing and drying bovine keratin as a raw material.

[0071] The modified animal protein foaming agent preparation method comprises: placing animal protein and 10-undecenoyl chloride in water, stirring at 50° C. for 3.5 hours, adjusting the pH value with hydrochloric acid until precipitation is generated, and then centrifuging and washing to obtain the modified animal protein foaming agent.

[0072] In terms of weight, the ultrafine powder includes 80 weight parts of fly ash, 40 weight parts of slag powder, 20 weight parts of desulfurized gypsum, 8 weight parts of silica fume and 8 weight parts of quicklime. 130 parts are taken and added to the concrete.

[0073] The average particle size of the fly ash particles is 5 μm.

[0074] The average particle size of the slag powder is 6 μm.

[0075] The specific surface area of ​​the silica fume is 18000m 2 / kg.

[0076] The average particle size of the quicklime particles is 12 μm.

[0077] The steps of preparing the concrete include:

[0078] 1) First, add the modified animal protein foaming agent into a foaming machine, add 210 parts by weight of water, generate foam, and set aside;

[0079] 2) Mix cement and ultrafine powder evenly, then add water, stir for 4 minutes, then add organic additives, stir for 1.5 minutes, then add the foam obtained in step 2) while stirring, stir for 25 seconds, pour the material into a mold and let it stand for 1 day, perform standard curing after demoulding, and obtain ultra-lightweight foamed concrete.

[0080] The standard curing is specifically as follows: standard curing for 28 days, during which the temperature is maintained at 20° C. and the humidity is 98%.

[0081] Example 3

[0082] This embodiment provides an ultra-lightweight foamed concrete. The raw materials for preparing the concrete include, by weight: 500 parts by weight of cement, 250 parts by weight of ultrafine powder, 50 parts by weight of organic additives, 21 parts by weight of foam, and 380 parts by weight of water.

[0083] In parts by weight, the organic auxiliary agent includes 11.3 parts by weight of trimesoyl chloride, 24.2 parts by weight of 1,8-octanediamine and 14.5 parts by weight of sodium bicarbonate.

[0084] In parts by weight, the raw materials for preparing the modified animal protein foaming agent include 40 parts by weight of animal protein, 6 parts by weight of 10-undecenoyl chloride and 90 parts by weight of water.

[0085] The animal protein is obtained by hydrolyzing and drying bovine keratin as a raw material.

[0086] The modified animal protein foaming agent preparation method comprises: placing animal protein and 10-undecenoyl chloride in water, stirring at 70° C. for 2.5 hours, adjusting the pH value with hydrochloric acid until precipitation is generated, and then centrifuging and washing to obtain the modified animal protein foaming agent.

[0087] In parts by weight, the ultrafine powder includes 160 parts by weight of fly ash, 80 parts by weight of slag powder, 40 parts by weight of desulfurized gypsum, 16 parts by weight of silica fume and 16 parts by weight of quicklime. 250 parts are taken and added to the concrete.

[0088] The average particle size of the fly ash is 12 μm.

[0089] The average particle size of the slag powder is 15 μm.

[0090] The specific surface area of ​​the silica fume is 25000m 2 / kg.

[0091] The average particle size of the quicklime particles is 15 μm.

[0092] The steps of preparing the concrete include:

[0093] 1) Add the modified animal protein foaming agent into a foaming machine, add 1200 parts by weight of water, generate foam, and set aside;

[0094] 2) Mix cement and ultrafine powder evenly, then add water, stir for 8 minutes, then add organic additives, stir for 1.5 minutes, then add the foam obtained in step 2) while stirring, stir for 40 seconds, pour the material into a mold and let it stand for 1 day, perform standard curing after demoulding, and obtain ultra-lightweight foamed concrete.

[0095] The standard curing is specifically as follows: standard curing for 28 days, during which the temperature is maintained at 20° C. and the humidity is 98%.

[0096] Example 4

[0097] The method is basically the same as Example 1, except that, in parts by weight, the organic auxiliary agent includes 9 parts by weight of trimesoyl chloride, 5.4 parts by weight of 1,9-nonanediamine and 10 parts by weight of sodium bicarbonate.

[0098] Example 5

[0099] The method is basically the same as Example 1, except that, in parts by weight, the reaction raw materials of the organic auxiliary agent include 9 parts by weight of trimesoyl chloride, 26.8 parts by weight of 1,9-nonanediamine and 10 parts by weight of sodium bicarbonate.

[0100] Example 6

[0101] The method is basically the same as Example 1, except that calcium hydroxide is used instead of sodium bicarbonate as the acid binding agent.

[0102] Comparative Example 1

[0103] The method is basically the same as Example 1, except that commercially available polyamide resin is used instead of the organic additive.

[0104] The commercially available polyamide resin is from Jiangsu Qiangsheng Functional Chemical Co., Ltd., and the model is 651. The polyamide resin does not contain a benzene ring structure.

[0105] Comparative Example 2

[0106] The method is basically the same as Example 1, except that dimethylmalonyl chloride (CAS No.: 5659-93-8) is used instead of trimesoyl chloride.

[0107] Comparative Example 3

[0108] The method is basically the same as Example 1, except that lauroyl chloride is used instead of 10-undecenoyl chloride.

[0109] Comparative Example 4

[0110] The method is basically the same as Example 1, except that 1,2-propylenediamine is used instead of 1,9-nonanediamine.

[0111] Comparative Example 5

[0112] This comparative example provides an ultra-lightweight foamed concrete and a preparation method thereof. The specific implementation method is the same as that of Example 1; the difference is that acryloyl chloride is used instead of 10-undecenoyl chloride.

[0113] Performance testing method:

[0114] Refer to JG / T266-2011 "Foamed Concrete" to conduct relevant mechanical strength and bulk density tests. Among them, the compressive strength test method after corrosion is: soak the concrete sample after curing for 28 days in a sodium sulfate aqueous solution with a mass concentration of 5%, and test the compressive strength after soaking for 90 days.

[0115] Performance test data:

[0116] The test results are shown in Table 1 below.

[0117] Table 1

[0118]

[0119]

[0120] Result analysis:

[0121] It can be seen from the test results that the ultra-lightweight foamed concrete prepared in Examples 1 to 6 has excellent mechanical properties and corrosion resistance, and a low bulk density. The performance of Example 1 is the most excellent.

[0122] Compared with Example 1, the compressive strength, corrosion resistance and bulk density of Example 4 are all deteriorated. The reason may be that when the amount of 1,9-nonanediamine added in the organic additive is too small, the degree of crosslinking becomes small, and the excess acyl chloride groups are hydrolyzed to form carboxyl groups, resulting in a loose polymer network structure. The loose structure is difficult to resist the invasion of sulfate ions and is not conducive to the traction and arrangement of the foam, thereby making the foam arrangement in the system disordered and the liquid film stability reduced. Therefore, the compressive strength and corrosion resistance of the obtained product are reduced, and the bulk density is increased.

[0123] Compared with Example 1, the compressive strength, corrosion resistance and bulk density of Example 5 are also relatively poor. The reason may be that when too much 1,9-nonanediamine in the organic additive is added, the benzene ring structure in the polymer structure is reduced, the overall cross-linking density is reduced, and the three-dimensional network structure with low supporting force is not only not conducive to the construction of pores, but also not conducive to compensating for the shrinkage of concrete. Therefore, the corrosion resistance of the product is reduced, the compressive strength is reduced, and the bulk density is increased.

[0124] Compared with Example 1, the compressive strength and corrosion resistance of Example 6 are higher, and the bulk density is larger. The reason may be that calcium hydroxide cannot produce carbon dioxide while binding acid, and builds a pore structure in a coordinated physical foaming manner. Compared with Example 1, the bulk density of the obtained product is significantly increased, and it is impossible to maintain light weight.

[0125] Compared with Example 1, the various properties of the product of Comparative Example 1 are all deteriorated, and the reason may be that: the commercially available polyamide resin is directly added instead of the organic additive. Compared with the organic additive of the present application, the interface bonding force between it and the inorganic material in the system is insufficient. When the green body is formed and subjected to load, the actual non-uniformity of the force causes the organic-inorganic interface to crack easily. In addition, the direct addition method cannot directly form a three-dimensional network structure in the system during the concrete preparation process, and it is difficult to form an effective skeleton support. Therefore, the compressive strength and corrosion resistance of the product are significantly reduced. In addition, due to the lack of carbon dioxide production, it is difficult to compensate for the foam and the bulk density increases.

[0126] Compared with Example 1, the compressive strength and corrosion resistance of the product obtained in Comparative Example 2 are both reduced. It is speculated that due to the chemical structure characteristics of dimethylmalonyl dichloride (no benzene ring), the supporting force is reduced, the steric hindrance of the organic additive is reduced, and the long chain entanglement phenomenon is easy to occur, resulting in reduced dispersibility of the components in the system, and unable to maintain a uniform and stable network structure, so the compressive strength and corrosion resistance of the product are reduced.

[0127] Compared with Example 1, the compressive strength and corrosion resistance of the product obtained in Comparative Example 3 are significantly reduced. The reasons are speculated to be: lauroyl chloride replaces 10-undecenoyl chloride, and its hydrophobic long chain is grafted onto the protein molecular chain, which improves the surface activity of the foaming agent, but reduces its foam stability; although the organic additive in the system can improve its foam stabilizing effect, lauroyl chloride cannot react with the polymer formed by the organic additive, so it has little effect on the orderly arrangement of bubbles, so the internal pore distribution of the product is uneven, the compressive strength of the product decreases, and the bulk density increases.

[0128] Compared with Example 1, the compressive strength and corrosion resistance of the product obtained in Comparative Example 4 are significantly reduced. The reason may be that when 1,2-propylenediamine is used to replace 1,9-nonanediamine, the chain length of 1,2-propylenediamine is too short, and the steric hindrance of trimesoyl chloride is relatively high, which affects the overall grafting density, resulting in a loose cross-linking network of the organic additive, so the compressive strength and corrosion resistance of the product are significantly reduced.

[0129] Compared with Example 1, the compressive strength and corrosion resistance of the product obtained in Comparative Example 5 are significantly reduced, and the bulk density is increased. Analysis shows that: on the one hand, the acryloyl chloride chain segment is relatively short, which does not improve the surface activity of the foaming agent well and the amount of foaming is small; on the other hand, the short-chain acryloyl chloride is difficult to be well grafted to the polymer structure formed by the organic additive, and it is difficult to improve the orderly arrangement of the foam, which is not helpful for the stability of the foam, resulting in the deterioration of the overall compressive strength, corrosion resistance and bulk density.

[0130] A comprehensive comparison of these experimental results shows that only by using the preferred organic additives of the present invention, the foam prepared by the modified animal protein foaming agent and the ultrafine powder together can the high strength, low quality and corrosion resistance of concrete be taken into account. The final concrete has high compressive strength, corrosion resistance retention rate and low bulk density, which meets the requirements of building materials.

Claims

1. An ultra-lightweight foaming concrete, characterized in that: The raw materials for preparing the concrete include, by weight: 250-500 parts of cement, 130-250 parts of ultrafine powder, 10-70 parts of organic additives, 6-27 parts of foam, and 190-380 parts of water; the organic additives include trimesoyl chloride and diamine.

2. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The diamine is a C3-C15 diamine; preferably, the diamine is a C6-C10 diamine.

3. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The molar ratio of trimesoyl chloride to diamine is 1:(1-5); preferably, the molar ratio of trimesoyl chloride to diamine is 1:(2-4).

4. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The diamine is at least one selected from 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine.

5. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The organic auxiliary agent also includes an acid binding agent; the acid binding agent includes at least one of calcium hydroxide, triethylamine, sodium carbonate, potassium carbonate, sodium acetate, and sodium bicarbonate.

6. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The foam is prepared by adding water to a modified animal protein foaming agent for foaming; the raw materials for preparing the modified animal protein foaming agent include animal protein, unsaturated acid chloride, and water in a mass ratio of 1: (0.05-0.5): (1-10); The preparation method of the modified animal protein foaming agent is as follows: animal protein, unsaturated acyl chloride and water are mixed, stirred at 40-80° C. for 2-5 hours, the pH value of the mixed solution is adjusted with hydrochloric acid until precipitation occurs, centrifuged, washed and dried to obtain the modified animal protein foaming agent.

7. The ultra-lightweight foamed concrete according to claim 6, characterized in that: The unsaturated acyl chloride is an unsaturated aliphatic acyl chloride; preferably, the unsaturated acyl chloride is an unsaturated aliphatic acyl chloride with a terminal olefin.

8. The ultra-lightweight foamed concrete according to claim 6, characterized in that: The unsaturated acid chloride is 10-undecenoyl chloride.

9. The ultra-lightweight foamed concrete according to claim 1, characterized in that: The mass ratio of the organic additive to the foam is 1:(0.2-0.6).

10. A method for preparing ultra-lightweight foamed concrete according to any one of claims 1 to 9, characterized in that: The steps of preparing the concrete include: 1) Adding modified animal protein foaming agent and water into a foaming machine to generate foam for standby use; 2) Mix cement and ultrafine powder evenly, then add water, stir for 1-20 minutes, then add high molecular copolymer, stir for 0.5-5 minutes, then add foam obtained in step 1) while stirring, stir for 10-60 seconds, pour the material into a mold, let it stand for 1-5 days, then demould, perform standard curing after demoulding, and obtain ultra-lightweight foamed concrete.