Ecological low-carbon leveling flowing mortar for ground and preparation method thereof
Through the combination of modified gypsum and fibers, the problem of water absorption and expansion and insufficient mechanical strength of the gypsum base leveling mortar in humid environments is solved, and the mechanical strength and wear resistance of the mortar are improved, which is suitable for high-strength floor use.
Patent Information
- Application Number
- CN202411339237.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The leveling mortar on the gypsum base floor absorbs water and expands in humid environments, has a lower strength, and is not suitable for use on the ground with load-bearing loads and special requirements.
Modified gypsum and modified composite fibers are used to add natural oils such as flaxseed oil, peanut oil, soybean oil, and polyurethane and epoxy resins to form a film that prevents moisture penetration, enhances the binding force of gypsum particles, and adds lignin fibers and polypropylene. Mesh fibers and carbon fibers improve mechanical properties and improve the binding force between fibers and mortar by cationically modified polyvinyl alcohol.
It significantly reduces the water absorption and shrinkage of the mortar, improves mechanical strength, freeze-thaw resistance and wear resistance, and meets the needs of high-strength floor use.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of building materials, and relates to an ecological low-carbon leveling flowing mortar for the ground and a preparation method thereof, and specifically to an ecological low-carbon leveling flowing mortar for the ground with low water absorption, high wear resistance and high mechanical strength and a preparation method thereof. Background Art
[0002] Floor leveling mortar plays a very important role in construction. It is mainly used to level the ground and provide a flat and solid foundation for subsequent floor laying or other surface treatments (such as tiles, wooden floors, carpets, etc.). The use of floor leveling mortar can effectively solve the problems caused by uneven foundation or uneven settlement, improve the quality of the building and extend the service life of the floor material. According to different use conditions and requirements, floor leveling mortar can generally be divided into the following types: cement-based leveling mortar, gypsum-based leveling mortar, self-leveling mortar, etc. Among them, cement-based leveling mortar is the most common leveling method, which is composed of cement, fine aggregate (such as sand), additives, etc., and is suitable for most indoor floor leveling projects; gypsum-based leveling mortar has good thermal insulation performance, and dries quickly, which is suitable for fast construction; self-leveling mortar is a special leveling material with very good fluidity. It can automatically flow and level the ground, which is particularly suitable for ground projects that require high-precision flatness.
[0003] As a traditional building material, cement-based leveling mortar is mainly made of cement and fine aggregates. However, a large amount of carbon dioxide is released during the cement production process, mainly because the decomposition of limestone produces carbon dioxide. Therefore, the production and use of cement will produce greenhouse gases, affecting carbon emissions. In addition, cement manufacturing is a high-energy consumption process. From the mining of raw materials to the manufacture of final products, a large amount of energy is consumed. High energy consumption means higher use of chemical fuels, which in turn exacerbates the problem of carbon emissions. Therefore, cement-based leveling mortar has shortcomings in terms of green environmental protection and low carbon.
[0004] In order to mitigate these negative impacts, the construction industry is constantly exploring more environmentally friendly and low-carbon alternatives. Compared with traditional cement, the production process of gypsum releases less carbon dioxide. The production energy consumption of gypsum-based materials is relatively low, and it does not require high-temperature calcination like cement. Therefore, the energy demand and carbon emissions of gypsum-based materials are lower than those of cement products. Gypsum-based leveling mortar is not only green and low-carbon, but also has good thermal insulation, recyclability and fast hardening.
[0005] Although gypsum-based floor leveling mortar has many advantages in terms of green environmental protection, low carbon and thermal insulation performance, in actual application, due to the high sensitivity of gypsum-based materials to moisture, long-term exposure to humid environment, the gypsum-based leveling layer may absorb water and expand, resulting in strength loss or even powdering. In addition, compared with cement-based materials, gypsum-based floor leveling mortar has lower mechanical strength and is not suitable for load-bearing and special requirements. Summary of the invention
[0006] In view of the problem that the current gypsum-based floor leveling mortar has poor waterproof performance and mechanical properties, the purpose of this application is to provide an ecological low-carbon floor leveling mobile mortar and a preparation method thereof. The mortar of the present invention uses gypsum as the main material, and the gypsum is modified and combined with modified composite fibers, which not only ensures the green and low-carbon nature of the floor leveling mortar, but also improves the mechanical strength, freeze-thaw resistance and wear resistance of the mortar, reduces water absorption and shrinkage, and improves the comprehensive performance of the mortar.
[0007] The present application provides an ecological low-carbon leveling flowing mortar for the ground, characterized in that it comprises the following raw materials in parts by weight:
[0008] Modified gypsum 30~60 parts
[0009] Modified composite fiber 3~5 parts
[0010] 4~5 parts of filler
[0011] Aggregate 25~45 parts
[0012] 1~3 parts of glue powder
[0013] Water reducing agent 0.04~0.0.6 parts
[0014] Thickener 0.01~0.05 parts
[0015] Retarder 0.01~0.05 parts
[0016] Leveling agent 0.05~0.15 parts
[0017] 10-20 parts water;
[0018] The preparation method of modified gypsum is:
[0019] S11: mixing fluorinated gypsum, phosphogypsum and hemihydrate gypsum evenly to obtain mixed gypsum for later use;
[0020] S12: adding linseed oil, peanut oil, soybean oil and dibenzoyl peroxide into water to form a first dispersion liquid for later use;
[0021] S13: adding polyurethane and epoxy resin into water to form a second dispersion for later use;
[0022] S14: adding the first dispersion to the mixed gypsum and mixing evenly, then adding the second dispersion and stirring for 3-5 hours, filtering and drying to obtain modified gypsum;
[0023] The preparation method of the modified composite fiber is as follows:
[0024] S21: mixing lignin fiber, polypropylene mesh fiber and carbon fiber uniformly to obtain mixed fiber, soaking the mixed fiber in a 5-8% sulfuric acid aqueous solution for 8-10 hours, taking out, washing and drying to obtain activated fiber for standby use;
[0025] S22: adding polyvinyl alcohol to isopropanol and stirring, then slowly dropping a sodium hydroxide aqueous solution with a concentration of 0.1-0.5% under stirring, raising the temperature to 50-60° C. and maintaining for 1-1.5 hours, continuing to drop glycidyl dimethyl behenyl ammonium chloride and reacting for 4-6 hours, precipitating a product, neutralizing with hydrochloric acid to adjust the pH value to 7, washing and soaking with acetone to remove residual reactants, and drying at 30-50° C. for 4-6 hours to obtain a cation-modified polyvinyl alcohol for standby use;
[0026] S23: Put the activated fiber into a reactor, add water, then add cationic modified polyvinyl alcohol and stir evenly, raise the temperature to 60-80°C and react for 30-60 minutes. After the reaction is completed, filter, wash and dry to obtain modified composite fiber.
[0027] At present, leveling mortar is divided into wall leveling mortar and ground leveling mortar according to its different uses. Wall leveling mortar is used for walls, and it mainly bears the weight in the vertical direction and possible lateral stress. Ground leveling mortar is mainly used for the ground, and it needs to bear the pressure and impact caused by walking, furniture movement and equipment placement. Therefore, although they are all leveling mortars, due to different application scenarios, compared with wall leveling mortar, ground leveling mortar requires mortar with higher strength and higher wear resistance. Based on low-carbon and environmental protection, the present invention uses gypsum as the main material. In view of the high water absorption and poor strength of gypsum, the present invention modifies the gypsum, reduces the water absorption rate of gypsum, and improves the mechanical strength of the mortar. Analysis of the reasons: In the preparation process of modified gypsum, natural oils such as linseed oil, peanut oil and soybean oil are added. These ingredients can form a thin film on the surface of gypsum particles. This film can prevent the rapid penetration of water, thereby reducing the water absorption rate of the mortar. At the same time, polyurethane and epoxy resin form a second dispersion liquid that can react with gypsum particles, enhance the bonding force between gypsum particles, reduce the number and size of pores, and further reduce water absorption. The introduction of modifiers causes changes in the growth mode of gypsum crystals, and may form a denser crystal structure, which can reduce the voids inside the mortar, thereby reducing the absorption of water. The addition of epoxy resin and polyurethane can also form a fine network structure during the hardening process, fill the gaps between the gypsum hydration products, improve the density of the mortar, and reduce water absorption. The present invention makes the hydration process of gypsum more uniform through modification, reduces the local shrinkage differences caused by uneven hydration, and thus reduces the overall shrinkage rate. Organic materials such as polyurethane and epoxy resin can form elastomers during the hardening process, and the presence of these elastomers can absorb part of the stress caused by shrinkage, prevent cracking, and thus reduce shrinkage.
[0028] In order to improve the mechanical strength of the ground leveling flowing mortar, the present invention adds lignin fiber, polypropylene mesh fiber and carbon fiber, which significantly improves the mechanical properties of the mortar. Wherein the lignin fiber and the polypropylene mesh fiber have a high tensile strength, and they play a "bridging" role in the mortar, can effectively disperse and transfer tensile stress, thereby improving the tensile strength of the mortar and reducing the risk of cracking. The polypropylene mesh fiber also has a certain elasticity and toughness, can absorb energy when the mortar is impacted, reduce the occurrence and development of cracks, and improve the impact resistance of the mortar. Carbon fiber has very high strength and modulus, and its addition can significantly improve the bending strength of the mortar, especially when subjected to bending loads, can better resist deformation and fracture. The hardness of carbon fiber is high, which can significantly improve the wear resistance of the mortar, especially in high wear areas, such as the ground with a large flow of people, can extend the service life of the mortar. Lignin fiber and polypropylene mesh fiber can also reduce the chance of direct contact between the wear medium and the mortar by filling the tiny pores in the mortar, thereby indirectly improving the wear resistance.
[0029] The inventors continued to study and found that although the addition of lignin fiber, polypropylene mesh fiber and carbon fiber can improve the mechanical properties of the mortar to a certain extent, the above three fibers have poor dispersibility in the mortar and are easy to form agglomerates. The bonding force between the fiber and the mortar body is poor. In the long-term use process, in a humid environment or in a freeze-thaw environment, it is very easy for the mechanical properties to decline. In response to this problem, the present invention activates and modifies the three fibers. Specifically, the activated fiber is modified with cationic modified polyvinyl alcohol. Cationic modified polyvinyl alcohol can improve the interfacial bonding force between the fiber and the mortar material, thereby improving the durability of the mortar. Analysis of the reasons: The modified fiber has better bonding with the mortar matrix, can more effectively disperse stress, and reduce the formation of microcracks caused by freeze-thaw cycles. Cationic modified PVA can help the fiber to be evenly dispersed in the mortar, reduce porosity, and increase the density of the mortar, thereby reducing the chance of water entering the mortar and reducing freeze-thaw damage. The good interface bonding between the modified composite fiber and the mortar body reduces the risk of debonding between the fiber and the matrix, making the mortar less prone to deterioration during long-term use and maintaining good physical and mechanical properties. The stable distribution of the modified fiber in the mortar can effectively resist external stress, improve the tensile, bending and impact resistance of the mortar, and thus extend its service life.
[0030] In some embodiments of the present application, the mass ratio of fluorgypsum, phosphogypsum and hemihydrate gypsum is (3-5): (0.5-2): (10-15);
[0031] The mass ratio of linseed oil, peanut oil and soybean oil is (2-4):1:1, the amount of dibenzoyl peroxide added is 0.5-1% of the mass of linseed oil, and the mass ratio of the total mass of linseed oil, peanut oil, soybean oil and dibenzoyl peroxide to water is 1:20-30;
[0032] The mass ratio of polyurethane to epoxy resin is (8-10):1, the viscosity of polyurethane is ≤500mpa•s, the epoxy equivalent of epoxy resin is 400-800, the viscosity is >2000mpa•s, and the mass ratio of the total mass of polyurethane and epoxy resin to water is 1:(35-40);
[0033] The mass of the linseed oil in the first dispersion is 0.5-0.8% of the total mass of the mixed gypsum, and the mass of the polyurethane in the second dispersion is 0.1-0.3% of the total mass of the mixed gypsum.
[0034] Polyurethane was purchased from Anhui Yuanchen New Materials Technology Co., Ltd., model number is YC-612.
[0035] Epoxy resin was purchased from Shenzhen Jitian Chemical Co., Ltd., model F0705.
[0036] In the present invention, the mixing of fluorinated gypsum, phosphogypsum and hemihydrate gypsum in different proportions can make the final modified gypsum have better hydration characteristics and mechanical properties, thereby helping to control water absorption and shrinkage. Different types of gypsum will exhibit different behaviors when hydrated. By adjusting their proportions, a balance point can be reached, so that the mortar will neither crack due to excessive expansion nor affect strength due to excessive shrinkage during the hardening process.
[0037] The present invention defines the ratio of linseed oil, peanut oil and soybean oil. Within this ratio range, the modified gypsum can be ensured to have good fluidity and self-compactness, making it easy to lay and level during construction, promoting the formation of a stable network structure, and improving the compressive strength and flexural strength of the modified gypsum. An inappropriate ratio of the three vegetable oils may affect the formation of the internal structure of the modified gypsum, resulting in a decrease in its compressive and flexural strengths. An inappropriate ratio may also lead to uneven distribution of internal stress after the mortar hardens, making it prone to cracking.
[0038] The present invention limits the ratio of polyurethane and epoxy resin and the viscosity parameters of both. Under this ratio range, suitable ratio and viscosity can ensure that polyurethane and epoxy resin form an effective network structure in modified gypsum, thereby improving the compressive strength, flexural strength and toughness of mortar, helping to form stable chemical bonds, reducing the pores inside the mortar, and improving its durability and chemical stability. Moderate viscosity also helps mortar to have good fluidity and self-compactness during construction, is convenient for construction, and ensures that the mortar surface is smooth. If the viscosity is too high, the mortar will become too thick, poor fluidity, and difficult to construct, which may cause mortar to be layered or segregated during laying. Too low viscosity may cause the mortar to be too thin and unable to maintain shape, affecting the molding effect. In addition, improper viscosity or ratio may cause the internal porosity of the mortar to increase, and moisture is more likely to invade, reducing its freeze-thaw resistance.
[0039] In some embodiments of the present application, the mass ratio of lignin fiber, polypropylene mesh fiber and carbon fiber is (0.1-0.3): (0.5-0.8): 1;
[0040] The viscosity of polyvinyl alcohol is 80-110 mPa•s, and the alcoholysis degree is 87-89 mol%; polyvinyl alcohol was purchased from Shanghai Kaiyin Chemical Co., Ltd., and the model is PVA-235.
[0041] The mass ratio of polyvinyl alcohol, isopropanol and sodium hydroxide aqueous solution is 1:(4-6):(2-3), and the mass ratio of polyvinyl alcohol and glycidyl dimethyl behenyl ammonium chloride is 1:(0.5-0.8);
[0042] The mass ratio of activated fiber, cationic modified polyvinyl alcohol and water is (30~50):1:(150~200).
[0043] The present invention defines the mass ratio of lignin fiber, polypropylene mesh fiber and carbon fiber. Within this ratio range, the appropriate ratio of the three fibers can ensure that the fibers are evenly distributed in the mortar, give full play to their reinforcing effect, and improve the overall tensile, compressive and flexural strength of the mortar. By adjusting the fiber ratio, the microstructure of the mortar can be optimized so that it can better disperse stress when subjected to force and reduce the generation of cracks. The uniform distribution of fibers can reduce microcracks inside the mortar, thereby improving its durability. The presence of fibers can also reduce water penetration and reduce damage caused by freeze-thaw cycles. If the ratio of the three fibers changes, for example, the proportion of carbon fibers increases, too much carbon fibers may cause uneven strength distribution inside the mortar, and some areas become too hard due to fiber accumulation, while other areas may lack strength due to lack of fibers.
[0044] In some embodiments of the present application, the length of the lignin fiber is not greater than 6 mm, the oil absorption rate is not less than 5 to 8 times the mass of the fiber itself, the moisture content is <5%, the bulk density is 300 to 400 g / L, and it is purchased from Shenzhen Hengyueda Building Materials Co., Ltd., model KLW-005.
[0045] In some embodiments of the present application, the polypropylene mesh fiber has a density of 0.91 kg / m3, a length of 19 mm, an equivalent diameter of <100 μm, an elastic modulus of >3500 MPa, and a tensile strength of ≥660 MPa, and is purchased from Shenzhen Hengyueda Building Materials Co., Ltd., model KLW-007.
[0046] In some embodiments of the present application, the length of the carbon fiber is 0.8 mm, the carbon content is ≥ 93%, and the density is ≥ 1.76 g / m 3 , strength ≥ 3.5 Gpa, purchased from Shanghai Lishuo Composite Materials Co., Ltd., model LSCF0.8-S.
[0047] In some embodiments of the present application, the filler is at least one of calcium carbonate and fly ash.
[0048] In some embodiments of the present application, the aggregate is sand with a mesh size of 100 to 200.
[0049] In some embodiments of the present application, the rubber powder is a redispersible latex powder.
[0050] In some embodiments of the present application, the water reducer is a polycarboxylate high-efficiency water reducer.
[0051] In some embodiments of the present application, the thickener is cellulose ether, and the viscosity of the cellulose ether is 200-800 mpa•s.
[0052] In some embodiments of the present application, the retarder is a protein-based retarder; the leveling agent is at least one of polymethylphenylsiloxane and leveling agent 2041.
[0053] The present application provides a method for preparing ecological low-carbon leveling flowing mortar for ground use, the preparation method comprising the following steps:
[0054] S1: Weigh modified gypsum, modified composite fiber, filler, aggregate, rubber powder, water reducer, thickener and leveling agent in proportion and mix them in a mixer at 100-200 r / min for 3-8 min to obtain a mixture;
[0055] S2: Add water to the mixture, mix at 150-300 r / min for 2-6 minutes, stop for 1-30 minutes, and continue stirring for more than 3 minutes to obtain leveling flowing mortar.
[0056] Compared with the prior art, the present application at least achieves the following technical effects:
[0057] The present application relates to an ecological low-carbon leveling flowing mortar for the ground and a preparation method thereof. The prepared ground leveling mortar not only has the advantages of being green, environmentally friendly and low-carbon, but also has good waterproof performance and mechanical strength, low shrinkage rate, high wear resistance, and at least obtains the following technical effects:
[0058] (1) The present invention uses industrial byproducts fluorinated gypsum and phosphogypsum to replace natural gypsum, which not only reduces the exploitation of natural resources, but also finds new uses for industrial waste and realizes the effective recycling of resources. The production process of the present invention utilizes low-carbon technology and adopts mild chemical reaction conditions, which reduces energy consumption and thus reduces carbon dioxide emissions in the entire production process;
[0059] (2) The use of the modified gypsum and the modified composite fiber of the present invention significantly improves the compressive strength, flexural strength and wear resistance of the floor leveling mortar, which makes the finished product have better mechanical properties and mechanical strength, and can meet the high-strength floor use requirements;
[0060] (4) The floor leveling flowing mortar of the present invention has good fluidity and self-compacting properties, which means that it can automatically level, reduce the workload of manual leveling, and improve the construction speed. The leveling agent added in the present invention can make the mortar surface smoother, reduce the generation of bubbles and cracks, and finally form a beautiful and durable floor surface layer;
[0061] (5) The present invention uses industrial waste as raw materials to reduce the cost of raw materials, while the efficient production process reduces energy consumption and labor costs. Due to its excellent durability, the frequency of later repairs and renovations is reduced, which can save a lot of maintenance costs in the long run;
[0062] (6) The reasonable proportion and simplified preparation process of the present invention make on-site construction more convenient and quickly complete the mixing, laying and curing process of the mortar, which is conducive to shortening the construction period of the entire project. DETAILED DESCRIPTION
[0063] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below. However, it should be understood that the description herein is only used to explain the present invention and is not used to limit the scope of the present invention.
[0064] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention, and the terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The reagents and instruments used herein are all commercially available, and the characterization means involved can refer to the relevant descriptions in the prior art, which will not be repeated herein.
[0065] Example 1
[0066] An ecological low-carbon leveling flowing mortar for the ground comprises the following raw materials in parts by weight:
[0067] 50 parts of modified gypsum;
[0068] 5 parts of modified composite fiber;
[0069] 4.5 parts of filler; the filler is calcium carbonate;
[0070] 30 parts of aggregate; the aggregate is 100~200 mesh sand;
[0071] 2 parts of rubber powder; the rubber powder is redispersible latex powder purchased from Guangzhou Tongxin Chemical Co., Ltd.;
[0072] 0.05 parts of water reducing agent; the water reducing agent is a polycarboxylate high-efficiency water reducing agent purchased from Guangdong Meihua New Material Technology Co., Ltd., model PT-3210;
[0073] 0.03 parts of thickener; the thickener is cellulose ether, the viscosity of cellulose ether is 300-800 mpa•s, purchased from Sichuan Lanyang Daily Chemical Co., Ltd., model IM6;
[0074] 0.02 parts of retarder; the retarder is a protein retarder purchased from Wuhan Huaxuan High-tech Co., Ltd., model KH-GR802;
[0075] 0.1 part of leveling agent; the leveling agent is leveling agent 2041, purchased from Laiyang Shengbang Silicone Technology Co., Ltd.;
[0076] 15 parts water;
[0077] The preparation method of modified gypsum is:
[0078] S11: mixing fluorite, phosphogypsum and hemihydrate gypsum evenly to obtain mixed gypsum for standby use; the mass ratio of fluorite, phosphogypsum and hemihydrate gypsum is 4:1.5:12;
[0079] S12: adding linseed oil, peanut oil, soybean oil and dibenzoyl peroxide into water to form a first dispersion for later use; the mass ratio of linseed oil, peanut oil and soybean oil is 3:1:1, the amount of dibenzoyl peroxide added is 0.8% of the mass of linseed oil, and the mass ratio of the total mass of linseed oil, peanut oil, soybean oil and dibenzoyl peroxide to water is 1:25;
[0080] S13: adding polyurethane and epoxy resin into water to form a second dispersion for standby use; the mass ratio of polyurethane to epoxy resin is 9:1, the viscosity of polyurethane is ≤500mpa•s, polyurethane is purchased from Anhui Yuanchen New Material Technology Co., Ltd., model number is YC-612, epoxy equivalent of epoxy resin is 400-800, viscosity is>2000mpa•s, epoxy resin is purchased from Shenzhen Yoshida Chemical Co., Ltd., model number is F0705, and the mass ratio of the total mass of polyurethane and epoxy resin to water is 1:38;
[0081] S14: adding the first dispersion to the mixed gypsum and mixing evenly, then adding the second dispersion and stirring for 4 hours, filtering and drying to obtain modified gypsum; the mass of linseed oil in the first dispersion is 0.6% of the total mass of the mixed gypsum, and the mass of polyurethane in the second dispersion is 0.2% of the total mass of the mixed gypsum.
[0082] The preparation method of the modified composite fiber is as follows:
[0083] S21: The lignin fiber, polypropylene mesh fiber and carbon fiber are mixed evenly to obtain a mixed fiber, and the mixed fiber is soaked in a 6% sulfuric acid aqueous solution for 9 hours, then taken out, washed and dried to obtain activated fiber for standby use; the mass ratio of lignin fiber, polypropylene mesh fiber and carbon fiber is 0.2:0.6:1; the length of the lignin fiber is not more than 6 mm, the oil absorption rate is not less than 5-8 times the mass of the fiber itself, the moisture content is <5%, the bulk density is 300-400 g / L, purchased from Shenzhen Hengyueda Building Materials Co., Ltd., model KLW-005; the density of the polypropylene mesh fiber is 0.91 kg / m 3 , length is 19mm, equivalent diameter <100μm, elastic modulus>3500Mpa, tensile strength ≥660Mpa, purchased from Shenzhen Hengyueda Building Materials Co., Ltd., model KLW-007; carbon fiber length is 0.8mm, carbon content ≥93%, density ≥1.76g / m 3 , strength ≥ 3.5 Gpa, purchased from Shanghai Lishuo Composite Materials Co., Ltd., model LSCF0.8-S;
[0084] S22: Add polyvinyl alcohol to isopropanol and stir, then slowly drop a 0.3% sodium hydroxide aqueous solution under stirring, heat to 55°C and keep for 1.5 hours, continue to drop glycidyl dimethyl behenyl ammonium chloride and react for 5 hours, precipitate a product, neutralize with hydrochloric acid to adjust the pH value to 7, wash and soak with acetone to remove residual reactants, dry at 45°C for 5 hours to obtain a cation-modified polyvinyl alcohol for standby use; the viscosity of the polyvinyl alcohol is 80~110mpa•s, and the degree of alcoholysis is 87~89mol%. The polyvinyl alcohol is purchased from Shanghai Kaiyin Chemical Co., Ltd., model PVA-235; the mass ratio of polyvinyl alcohol, isopropanol and sodium hydroxide aqueous solution is 1:5:2, and the mass ratio of polyvinyl alcohol to glycidyl dimethyl behenyl ammonium chloride is 1:0.6;
[0085] S23: Put the activated fiber into a reactor, add water, then add cationic modified polyvinyl alcohol and stir evenly, heat to 65°C and react for 40 minutes. After the reaction is completed, filter, wash and dry to obtain modified composite fiber. The mass ratio of activated fiber, cationic modified polyvinyl alcohol and water is 40:1:150.
[0086] A method for preparing ecological low-carbon leveling flowing mortar for ground, comprising the following steps:
[0087] S1: Weigh modified gypsum, modified composite fiber, filler, aggregate, rubber powder, water reducer, thickener and leveling agent in proportion and mix them in a mixer at 150 r / min for 5 min to obtain a mixture;
[0088] S2: Add water to the mixture, mix at 200r / min for 4min, stop for 5min, and continue stirring for more than 3min to obtain leveling flowing mortar.
[0089] Example 2
[0090] The difference between this embodiment and embodiment 1 is that the formula of the ecological low-carbon leveling flowing mortar for the ground is different.
[0091] Ecological low-carbon leveling flowing mortar for the ground includes the following raw materials in parts by weight:
[0092] 55 parts of modified gypsum;
[0093] 4 parts of modified composite fiber;
[0094] 4 parts of filler;
[0095] Aggregate 42 parts;
[0096] 1 part of rubber powder;
[0097] 0.05 parts of water reducing agent;
[0098] Thickener 0.02 parts;
[0099] Retarder 0.02 parts;
[0100] 0.12 parts of leveling agent;
[0101] 20 parts water.
[0102] Comparative Example 1
[0103] The difference between this comparative example and Example 1 is that the mass ratio of fluorgypsum, phosphogypsum and hemihydrate gypsum in the preparation process of modified gypsum is 10:1.5:12.
[0104] Comparative Example 2
[0105] The difference between this comparative example and Example 1 is that linseed oil, peanut oil and soybean oil are not added during the preparation of the modified gypsum.
[0106] Comparative Example 3
[0107] The difference between this comparative example and Example 1 is that in the preparation process of the modified gypsum, the epoxy equivalent of the epoxy resin is 220-280, the viscosity is 1000 mpa•s, and it is purchased from Shenzhen Jitian Chemical Co., Ltd., model F0704.
[0108] Comparative Example 4
[0109] The difference between this comparative example and Example 1 is that the mass ratio of polyurethane to epoxy resin in the preparation process of modified gypsum is 9:5.
[0110] Comparative Example 5
[0111] The difference between this comparative example and Example 1 is that no polyurethane and epoxy resin are added during the preparation of the modified gypsum.
[0112] Comparative Example 6
[0113] The difference between this comparative example and Example 1 is that the mass ratio of lignin fiber, polypropylene mesh fiber and carbon fiber in the preparation process of the modified composite fiber is 0.2:0.6:5.
[0114] Comparative Example 7
[0115] The difference between this comparative example and Example 1 is that the length of the carbon fiber in the preparation process of the modified composite fiber is 10 mm, the carbon content is ≥ 93%, and the density is ≥ 1.76 g / m 3 , strength ≥ 3.5 Gpa, purchased from Shanghai Lishuo Composite Materials Co., Ltd., model LS-CF10-S.
[0116] Comparative Example 8
[0117] The difference between this comparative example and Example 1 is that the mixed fiber is not activated with sulfuric acid during the preparation of the modified composite fiber.
[0118] Comparative Example 9
[0119] The difference between this comparative example and Example 1 is that the viscosity of the polyvinyl alcohol in the preparation process of the modified composite fiber is 40-48 mpa•s, the alcoholysis degree is 87-89 mol%, and the polyvinyl alcohol is purchased from Shanghai Kaiyin Chemical Co., Ltd., and the model is PVA-224.
[0120] Comparative Example 10
[0121] The difference between this comparative example and Example 1 is that during the preparation of the modified composite fiber, the activated fiber is not mixed with the cationic modified polyvinyl alcohol, but is directly added to the mortar as the modified composite fiber.
[0122] Comparative Example 11
[0123] The difference between this comparative example and Example 1 is that polyvinyl alcohol is directly mixed with the activated fiber during the preparation of the modified composite fiber, and polyvinyl alcohol is used instead of the cationic modified polyvinyl alcohol in Example 1.
[0124] Performance Testing
[0125] The results of performance testing of the embodiments and comparative examples according to the requirements of JC / T 985-2017 "cement-based self-leveling mortar for floor use" are shown in Table 1 below.
[0126] Impact resistance is divided into three levels: Level I means no cracking or detachment from the base plate, Level II means slight cracking upon careful observation, and Level III means obvious cracking.
[0127] The mortar prepared in the embodiment and the comparative example was placed at -20°C until it was frozen solid and kept for 3 hours, and then placed at room temperature until it dissolved into mortar and kept for 3 hours. This cycle was repeated 10 times to complete the freeze-thaw experiment of the mortar. After the experiment was completed, the 28d compressive strength of the mortar was tested in accordance with the requirements of JC / T 985-2017 "Cement-based self-leveling mortar for floor use", and the 28d compressive strength retention rate after cyclic freeze-thaw was calculated.
[0128] The compressive strength retention rate 28 days after freeze-thaw cycles = (compressive strength 28 days before freeze-thaw cycles - compressive strength 28 days after freeze-thaw cycles) / compressive strength 28 days before freeze-thaw cycles × 100%.
[0129] The mortars prepared in the examples and comparative examples were subjected to a 28d compressive strength test in accordance with the requirements of JC / T 985-2017 "Cement-based self-leveling mortar for floor use". After the test, the cured mortars were placed in an environment with a humidity of 100% and a temperature of 50°C for 15 days, and then their compressive strength was tested again, and the compressive strength retention rate after humid environment treatment was calculated.
[0130] Compressive strength retention rate after humid environment treatment = (compressive strength before humid environment treatment - compressive strength after humid environment treatment) / compressive strength before humid environment treatment × 100%.
[0131] Table 1 Comprehensive performance test results
[0132]
[0133] It can be seen from the above performance test results that the mortars prepared in Examples 1-2 not only have excellent mechanical strength, but also have the advantages of freeze-thaw resistance and low water absorption. In particular, the comprehensive performance of Example 1 is the most outstanding. This is mainly because gypsum is used as the main raw material in the present invention to prepare ground flow leveling mortar. In order to solve the problems of easy water absorption and low mechanical strength of gypsum, not only the gypsum is modified to reduce its water absorption, but also modified composite fibers are added to improve the mechanical strength of the mortar. The mortar prepared by the present invention has excellent comprehensive performance.
[0134] However, the comparative example is significantly inferior to the embodiment in the corresponding performance test because it does not adopt the necessary technical solutions. In comparative example 1, the ratio of the three types of gypsum in the modified gypsum is changed. From the results, it can be seen that the mechanical strength and freeze-thaw resistance of the mortar are reduced, which proves that there is a synergistic effect between the three types of gypsum, which has an important influence on improving the comprehensive performance of the mortar. In comparative example 2, the three types of vegetable oils were not added during the preparation of the modified gypsum. From the results, it can be seen that the mechanical strength and freeze-thaw resistance of the mortar are reduced. At the same time, after the mortar is cured and placed in a humid environment for a period of time, the mechanical strength is significantly reduced, which proves that the three types of vegetable oils can be coated on the surface of the gypsum and reduce the water absorption rate of the gypsum, indicating that the addition of vegetable oil has an important influence on improving the comprehensive performance of the mortar. In Comparative Example 3, the type of epoxy resin was changed. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the addition of epoxy resin can improve the comprehensive performance of the mortar to a certain extent. However, further limiting the type of epoxy resin can improve the comprehensive performance of the mortar to the best state. The type of epoxy resin plays a very important role in improving the performance of the mortar to the best. In Comparative Example 4, the ratio of polyurethane and epoxy resin was changed. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the ratio of polyurethane and epoxy resin has an important influence on improving the comprehensive performance of the mortar. In Comparative Example 5, polyurethane and epoxy resin were not added during the preparation of modified gypsum. From the results, it can be seen that compared with Comparative Example 4, the comprehensive performance of the mortar further decreased, indicating that the simultaneous addition of polyurethane and epoxy resin has a very important influence on improving the comprehensive performance of the mortar. In Comparative Example 6, the ratio of the three fibers was changed. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the ratio of the three fibers can work together to ensure the improvement of the comprehensive performance of the mortar. Once the amount of carbon fiber added increases, it will affect the comprehensive performance of the mortar, indicating that the ratio of the three fibers has an important influence on improving the performance of the mortar. In Comparative Example 7, the length of the carbon fiber was changed. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the parameters of the carbon fiber play an important role in improving the comprehensive performance of the mortar. In Comparative Example 8, the mixed fiber was not activated with sulfuric acid. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the activation of the mixed fiber can increase the reactive groups on the fiber surface, thereby increasing the reactivity of the fiber and increasing the compatibility of the fiber with other substances in the mortar. The activation of the mixed fiber has a very important influence on improving the comprehensive performance of the mortar. In Comparative Example 9, the viscosity of polyvinyl alcohol was changed. From the results, it can be seen that the comprehensive performance of the mortar decreased, indicating that the parameters of polyvinyl alcohol have a certain influence on improving the comprehensive performance of the mortar.Comparative Example 10 directly adds the activated fiber to the mortar without mixing it with the cation-modified polyvinyl alcohol. From the results, it can be seen that compared with Comparative Example 9, the comprehensive performance of the mortar is further reduced, indicating that the mixing of activated fiber and cation-modified polyvinyl alcohol has a very important influence on improving the comprehensive performance of the mortar. Comparative Example 11 changes the type of cation-modified polyvinyl alcohol and directly mixes the activated fiber with polyvinyl alcohol. From the results, it can be seen that the comprehensive performance of the mortar is reduced, indicating the necessity of mixing the activated fiber with cation-modified polyvinyl alcohol, which has an important influence on improving the performance of the mortar. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effect.
[0135] The applicant declares that this application uses the above-mentioned embodiments to illustrate a kind of ecological low-carbon leveling flowing mortar for the ground and its preparation method, but this application is not limited to the above-mentioned embodiments, that is, it does not mean that this application must rely on the above-mentioned embodiments to be implemented. The technicians in the relevant technical field should understand that any improvement to this application, the equivalent replacement of the raw materials of the product of this application, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of this application.
[0136] The preferred embodiments of the present application are described in detail above; however, the present application is not limited to the specific details in the above embodiments. Within the technical concept of the present application, a variety of simple modifications can be made to the technical solution of the present application, and these simple modifications all fall within the protection scope of the present application.
[0137] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not further describe various possible combinations.
Claims
1. An ecological low-carbon leveling flowing mortar for the ground, characterized by: The following raw materials are included in parts by weight: Modified gypsum 30~60 parts Modified composite fiber 3~5 parts 4~5 parts of filler Aggregate 25~45 parts 1~3 parts of glue powder Water reducing agent 0.04~0.0.6 parts Thickener 0.01~0.05 parts Retarder 0.01~0.05 parts Leveling agent 0.05~0.15 parts 10-20 parts water; The preparation method of modified gypsum is: S11: mixing fluorinated gypsum, phosphogypsum and hemihydrate gypsum evenly to obtain mixed gypsum for later use; S12: adding linseed oil, peanut oil, soybean oil and dibenzoyl peroxide into water to form a first dispersion, which is set aside; S13: adding polyurethane and epoxy resin into water to form a second dispersion for later use; S14: adding the first dispersion to the mixed gypsum and mixing evenly, then adding the second dispersion and stirring for 3-5 hours, filtering and drying to obtain modified gypsum; The preparation method of the modified composite fiber is as follows: S21: mixing lignin fiber, polypropylene mesh fiber and carbon fiber uniformly to obtain mixed fiber, soaking the mixed fiber in a 5-8% sulfuric acid aqueous solution for 8-10 hours, taking out, washing and drying to obtain activated fiber for standby use; S22: adding polyvinyl alcohol to isopropanol and stirring, then slowly dropping a sodium hydroxide aqueous solution with a concentration of 0.1-0.5% under stirring, raising the temperature to 50-60° C. and maintaining for 1-1.5 hours, continuing to drop glycidyl dimethyl behenyl ammonium chloride and reacting for 4-6 hours, precipitating a product, neutralizing with hydrochloric acid to adjust the pH value to 7, washing and soaking with acetone to remove residual reactants, and drying at 30-50° C. for 4-6 hours to obtain a cation-modified polyvinyl alcohol for standby use; S23: placing the activated fiber into a reactor, adding water, then adding cationic modified polyvinyl alcohol and stirring evenly, heating to 60-80° C. and reacting for 30-60 min. After the reaction is completed, filtering, washing and drying to obtain a modified composite fiber; The mass ratio of fluorite, phosphogypsum and hemihydrate gypsum is (3~5): (0.5~2): (10~15); The mass ratio of linseed oil, peanut oil and soybean oil is (2-4):1:1, the amount of dibenzoyl peroxide added is 0.5-1% of the mass of linseed oil, and the mass ratio of the total mass of linseed oil, peanut oil, soybean oil and dibenzoyl peroxide to water is 1:20-30; The mass ratio of polyurethane to epoxy resin is (8-10):1, and the mass ratio of the total mass of polyurethane and epoxy resin to water is 1:(35-40); The mass of linseed oil in the first dispersion is 0.5-0.8% of the total mass of the mixed gypsum, and the mass of polyurethane in the second dispersion is 0.1-0.3% of the total mass of the mixed gypsum; The mass ratio of lignin fiber, polypropylene mesh fiber and carbon fiber is (0.1~0.3):(0.5~0.8):1; The mass ratio of polyvinyl alcohol, isopropanol and sodium hydroxide aqueous solution is 1:(4-6):(2-3), and the mass ratio of polyvinyl alcohol and glycidyl dimethyl behenyl ammonium chloride is 1:(0.5-0.8); The mass ratio of activated fiber, cationic modified polyvinyl alcohol and water is (30~50):1:(150~200).
2. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The viscosity of polyurethane is ≤500mpa•s, the epoxy equivalent of epoxy resin is 400~800, and the viscosity is >2000mpa•s.
3. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The viscosity of polyvinyl alcohol is 80~110mpa•s, and the degree of alcoholysis is 87~89mol%.
4. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The filler is at least one of calcium carbonate and fly ash.
5. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The aggregate is 100~200 mesh sand.
6. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The rubber powder is redispersible latex powder.
7. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The water reducing agent is a polycarboxylate high efficiency water reducing agent.
8. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The thickener is cellulose ether, and the viscosity of cellulose ether is 200~800mpa•s.
9. The ecological low-carbon leveling flowing mortar for the ground according to claim 1 is characterized by: The retarder is a protein retarder; the leveling agent is at least one of polymethylphenylsiloxane and leveling agent 2041.
10. The method for preparing the ecological low-carbon leveling flowing mortar for the ground according to claim 1, characterized in that: The following steps are involved: S1: Weigh modified gypsum, modified composite fiber, filler, aggregate, rubber powder, water reducer, thickener and leveling agent in proportion and mix them in a mixer at 100-200 r / min for 3-8 min to obtain a mixture; S2: Add water to the mixture, mix at 150-300 r / min for 2-6 minutes, stop for 1-30 minutes, and continue stirring for more than 3 minutes to obtain leveling flowing mortar.
Citation Information
Patent Citations
Calcination-free chemical gypsum dry mixed mortar used for plastering on inner walls
CN101549985A
Self-leveling mortar as well as preparation method and application thereof
CN118063149A