Three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and preparation method thereof
By adopting a preparation method of three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal materials, the problems of harsh reaction conditions, poor reproducibility and low yield in the existing multi-dimensional Strandberg-type phosphorus molybdenum oxygen cluster crystal material preparation methods are achieved, and The efficient electrocatalytic activity and simple synthesis process improve the detection sensitivity of electrochemical sensors.
Patent Information
- Application Number
- CN202410869504.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
AI Technical Summary
The existing preparation methods of multi-dimensional Strandberg-type phosphorus molybdenum oxygen cluster crystal materials have the problems of harsh reaction conditions, poor reproducibility and low yield.
A method for preparing a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material is adopted, which includes dissolving H3PO3 and (NH4)6Mo7O24·4H2O in water, adjusting the pH value, adding praseodymium chloride and imidazole, and adjusting the pH to 4.0 with ammonia water. Heat treatment is performed to synthesize H2(NH4)3[C3N2H5][(PIIIO3)2Mo5O15]·4H2O crystal.
The excellent electrocatalytic activity of the phosphorus molybdenum oxygen cluster crystal material was achieved, the detection sensitivity of the electrochemical sensor was improved, the synthesis process was simplified, the reaction time was shortened, and white bulk crystals were obtained.
Smart Images

Figure CN118852015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and a preparation method thereof. Background Art
[0002] Polyoxometalates (abbreviated as polyoxometalates) are a class of polyoxometalate phosphomolybdenum oxometalate crystals that have attracted much attention. Their unique structure and diverse physical and chemical properties have made them widely used in catalysis, biomedicine, sensing and materials. Using polyoxometalates as building blocks to construct multidimensional crystalline materials has always been a hot topic in the research of polyoxometalate synthetic chemistry. As a special branch of polyoxometalates, Strandberg-type phosphomolybdenum oxometalates have attracted much attention due to their high electron density, easy modification and multiple coordination modes. They have obvious advantages in constructing multidimensional crystalline materials. In addition, Strandberg-type phosphomolybdenum oxometalates also have excellent electron storage and transmission capabilities and can undergo a series of continuous, rapid and reversible multi-electron redox processes without changing their structure. These characteristics give Strandberg-type phosphomolybdenum oxometalates unique advantages as efficient and stable electrocatalysts. At present, multidimensional Strandberg-type phosphomolybdenum oxometalate crystalline materials are mostly prepared by hydrothermal method, but it has the disadvantages of harsh reaction conditions, poor reproducibility and low yield. Therefore, a three-dimensional supramolecular structure phosphomolybdenum oxometalate crystalline material and its preparation method are proposed. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and a preparation method thereof, which solves the problems raised in the above background technology.
[0004] To achieve the above objectives, the present invention is implemented by the following technical solutions: a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material, including its chemical formula: H2(NH4)3[C3N2H5][(P III O3)2Mo5O 15 ]·4H2O, crystallized in monoclinic system, C2y space group, the specific structure of the phosphorus molybdenum oxygen cluster crystal material is described as follows: the phosphorus molybdenum oxygen cluster crystal consists of a [(P III O3)2Mo5O 15 ] 6- Anion, two [H] + , three [NH4] + , one [C3N2H5] + It consists of a cation and four crystal water molecules.
[0005] A method for preparing a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material comprises the following steps:
[0006] Step 1: Take H3PO3 and (NH4)6Mo7O 24 4H2O was dissolved in 20ml water;
[0007] Step 2: Adjust the pH value of the solution to 0.6 with hydrochloric acid;
[0008] Step 3: heating the obtained solution to 60°C, and adding praseodymium chloride and imidazole to the hot solution;
[0009] Step 4: The pH value of the solution was adjusted to 4.0 with aqueous ammonia, the solution was heated at 60°C for 30 minutes, the mixture was filtered and cooled to ambient temperature, and white block crystals were separated after 3 days.
[0010] Optionally, the step 1: taking H3PO3 and (NH4)6Mo7O 24 ·4H2O is dissolved in 20ml water, the amount of H3PO3 is 0.3g, 3.65mmol, (NH4)6Mo7O 24 The amount of 4H2O used is 1.235 g, 1.0 mmol.
[0011] Optionally, in the step 2: adjusting the pH value of the solution to 0.6 with hydrochloric acid, the molar concentration of HCl is 4 mol / L.
[0012] Optionally, in the step three, the obtained solution is heated to 60° C., and praseodymium chloride and imidazole are added to the hot solution, wherein the amount of praseodymium chloride used is 0.1 g, 0.695 mmol, and the amount of imidazole used is 0.1 g, 1.469 mmol.
[0013] Optionally, in step 4, the pH value of the solution is adjusted to 4.0 with NH3·H2O, the solution is heated at 60°C for 30 minutes, the mixture is filtered and cooled to ambient temperature, and the molar concentration of ammonia water in the process of separating white block crystals after 3 days is 1 mol / L.
[0014] The present invention provides a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and a preparation method thereof, which has the following beneficial effects:
[0015] The synthesized phosphorus molybdenum oxygen cluster crystal material has excellent electrocatalytic activity and can be used as an electrode modification material to effectively improve the detection sensitivity of electrochemical sensors and realize sensitive electrochemical detection of H2O2. The synthesis method of this crystal material has the advantages of simple synthesis, easy crystallization and short reaction time. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 For the present invention (a) [(P III O3)2Mo5O 15 ]6- Ball-and-stick model of anions (b) [(P III O3)2Mo5O 15 ] 6- Anion and [C3N2H5] + Cations and [NH4] + Coordination pattern diagram of ions;
[0017] Figure 2 For protonated imidazole [C3N2H5] + Cation and [(P III O3)2Mo5O 15 ] 6- Schematic diagram of the structure where the surface oxygen atoms of the anion form multi-point hydrogen bonds to form a three-dimensional framework;
[0018] Figure 3 This is the XRD spectrum of the phosphorus molybdenum oxygen cluster crystal material;
[0019] Figure 4 This is the infrared spectrum of the phosphorus molybdenum oxygen cluster crystal material;
[0020] Figure 5 This is a thermogravimetric curve of the phosphorus molybdenum oxygen cluster crystal material;
[0021] Figure 6 This is the UV-visible absorption spectrum of the phosphorus molybdenum oxygen cluster crystal material;
[0022] Figure 7 This is the energy dispersion spectrum of the phosphorus molybdenum oxygen cluster crystal material;
[0023] Figure 8 This is the cyclic voltammogram of the arsenic molybdenum oxygen cluster crystal material-CPE in 0.1mol / L H2SO4+0.1mol / L Na2SO4 solution;
[0024] Fig. 9 Comparison of cyclic voltammetry curves of phosphomolybdenum oxide cluster crystal-CPE at different scan rates;
[0025] Fig.10 Comparison of cyclic voltammetry curves of phosphorus molybdenum oxygen cluster crystal-CPE at different times;
[0026] Fig.11 This is a comparison of the cyclic voltammetry curves of the phosphorus molybdenum oxygen cluster crystal-CPE under different H2O2 concentrations;
[0027] Fig.12 This is the current-time response curve of the phosphomolybdenum oxygen cluster crystal-CPE to different concentrations of H2O2;
[0028] Fig.13This is a linear relationship diagram between the current response signal of the phosphomolybdenum oxygen cluster crystal-CPE and the H2O2 concentration. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0030] like Figures 1 to 13 As shown, the present invention provides a technical solution: a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material, including a chemical formula: H2(NH4)3[C3N2H5][(P III O3)2Mo5O 15 ]·4H2O, crystallized in monoclinic system, C2y space group, the specific structure of the material is described as follows: Single crystal X-ray diffraction research shows that the material consists of a [(P III O3)2Mo5O 15 ] 6- Anion, two [H] + , three [NH4] + , one [C3N2H5] + cation and four crystal water molecules (see Table 1). III O3)2Mo5O 15 The unit is composed of 5 {MoO6} octahedra and 2 {P III O3} units are combined by sharing bridging oxygen to form ( Figure 1 a), Mo VI The atoms adopt a six-coordination mode, and the Mo-O bond length is The P atom is located at {P III In the O3} pyramid geometry, the PO bond length is In addition, the protonated [C3N2H5] + Cations and crystal water molecules fill the adjacent {(P III O3)2Mo5O 15} units (POM) and form multi-point hydrogen bonding interactions with their surface oxygen atoms (OH···O POM : and NH···O POM : Forming a three-dimensional supramolecular structure ( Figure 2 ), this classical hydrogen bond is the main reason for stabilizing the supramolecular structure of phosphorus molybdenum oxygen cluster crystals.
[0031] A method for preparing a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material comprises the following steps:
[0032] Step 1: Take 0.3 g, 3.65 mmol, of H3PO3 and 1.235 g, 1.0 mmol, of (NH4)6Mo7O 24 4H2O was dissolved in 20ml water;
[0033] Step 2: Adjust the pH value of the solution to 0.6 with 4 mol / L hydrochloric acid;
[0034] Step 3: Heat the obtained solution to 60°C, add 0.1 g, 0.695 mmol, of PrCl3·6H2O and 0.1 g, 1.469 mmol, of imidazole to the hot solution;
[0035] The addition of PrCl3·6H2O is a key step in the synthesis of phosphorus molybdenum oxygen cluster crystals. 3+ ions do not appear in the crystal structure of the phosphomolybdenum oxygen cluster. However, when praseodymium chloride is not added during the synthesis process, crystals suitable for single crystal structure determination cannot be obtained. This shows that Pr 3+ Ions play an important role in directing chemical reactions and influencing the separation of crystalline products.
[0036] Step 4: The pH value of the solution was adjusted to 4.0 with 1 mol / L ammonia water, the solution was heated at 60°C for 30 minutes, the mixture was filtered and cooled to ambient temperature, and white block crystals were separated after 3 days.
[0037] Accurately weigh 0.01g of phosphorus molybdenum oxygen cluster crystals and grind them in an agate mortar, add 0.1g of graphite powder and grind for 30min, then add 0.1mL of paraffin oil as a binder and grind for 20min until a uniform mixture is formed, and fill the mixture into a quartz tube with an inner diameter of 2mm, with a packaging length of about 1.0-1.5cm. Insert a copper rod from the top of the quartz tube and contact the mixture in the quartz tube to prepare a carbon paste electrode modified with phosphorus molybdenum oxygen cluster crystal material (phosphorus molybdenum oxygen cluster crystal-CPE).
[0038] Example:
[0039] The prepared phosphorus molybdenum oxygen cluster crystals were subjected to X-ray powder diffraction (XRD) test ( Figure 3 The experimental XRD pattern of the phosphorus molybdenum oxygen cluster crystals is basically consistent with the main peak position in the simulated spectrum, which verifies the high purity of the prepared arsenic molybdenum oxygen cluster crystals.
[0040] The infrared spectrum of the phosphomolybdenum oxygen cluster crystal is shown in Figure 4 , at 992, 908, 796, 665 and 550 cm -1 The four characteristic absorption peaks at {(P III O3)2Mo5O 15} υ(PO), υ(Mo=Ot ),υ(Mo-O b -Mo) and υ(Mo-O c -Mo) stretching vibration. 2836-1052cm -1 The absorption peaks in the region correspond to the characteristic vibration peaks of imidazole ligands. -1 The band at 1662-1052 cm is attributed to the stretching vibration of υ(CH) -1 The strong absorption peak at 3138 cm is attributed to the δ(NH) and δ(CH) bending vibrations, υ(C=C) and υ(C=N) stretching vibrations of the imidazole ring. -1 The broad band at is the υ(OH) stretching vibration of the lattice water molecules.
[0041] In the temperature range of 30-800℃, the thermogravimetric curve of the phosphorus molybdenum oxygen cluster crystal undergoes a two-step weight loss process ( Figure 5 ), in the temperature range of 30-500 °C, the first weight loss is 14.82% (calculated as 14.60%), which is attributed to the release of imidazole ligands, three ammonia molecules and four lattice water molecules. When heated to 800 °C, the second weight loss is 11.47% (calculated as 12.23%), which is due to {H2P III 2Mo5O 21 The P2O3 and H2O produced by the decomposition of the cluster escaped, and the final product was MoO3. The total weight loss of 26.29% was consistent with the theoretical value of 26.83%.
[0042] The UV-visible spectra of the phosphomolybdenum oxide cluster crystals were measured in a pH 4.0 aqueous solution. Figure 6 ), two characteristic peaks appeared at 203 and 230nm in the wavelength range of 200-400nm, belonging to O b,c →Mo and O d →The charge transfer transition of Mo has a broad absorption peak at about 450nm, which is attributed to Mn 2+ d→d electron transfer transition of ions.
[0043] The energy dispersion spectrum confirms the presence of P, Mo, C, N and O elements in the phosphorus molybdenum oxygen cluster crystals ( Figure 7 );
[0044] Electrochemical performance test of phosphorus molybdenum oxygen cluster crystal-CPE:
[0045] The cyclic voltammetry (CV) curve of the phosphorus molybdenum oxygen cluster crystal-CPE was tested using a three-electrode system in a 0.1 mol / L H2SO4+0.1 mol / LNa2SO4 solution in the potential range of -0.8 to +0.6 V with a scan rate of 100 mV / s. Figure 8As shown, the CV curves show 4 quasi-reversible peaks with an average peak potential of E 1 / 2 =(E pa +E pc ) / 2 are -0.4745V(II′), -0.2965V(II-II′), 0.094V(III-III′) and 0.300V(IV-IV′), respectively, which are attributed to Mo VI The redox process at the center. When the scan rate is increased from 50 mV·s -1 Increase to 200mV·s -1 The current intensity of the cyclic voltammetry curve gradually increases. The peak current of II′ shows a good linear relationship with the scan rate, indicating that the redox process of the phosphorus molybdenum oxygen cluster crystal is a surface-controlled process ( Fig. 9 ).
[0046] The stability of phosphomolybdenum oxide cluster crystal-CPE in 0.1mol / L H2SO4+0.1mol / LNa2SO4 solution was investigated by monitoring the CV curve. Fig.10 As shown, the peak current remained almost unchanged after 24 h, which indicates that the PMO crystal-CPE has good stability in the electrolyte solution.
[0047] Fig.11 The cyclic voltammograms of the PMOO crystal-CPE in 0.1 mol / L H2SO4 + 0.1 mol / L Na2SO4 solution containing different concentrations of H2O2 are shown. After adding 0.1 mM H2O2, the I' and II' reduction peak currents increased significantly, indicating that the reduced species at the Mo center in the PMOO crystal have obvious electrocatalytic activity for H2O2 reduction.
[0048] -0.7 V was selected as the applied potential. In 0.1 mol / L H2SO4+0.1 mol / LNa2SO4 solution, 50 μM H2O2 was added every 45 s, and a fast and stable amperometric current response was obtained. Figure 12-13 As shown in the figure, the current response of the phosphorus molybdenum oxygen cluster crystal-CPE gradually increases with the increase of H2O2 concentration, and the response time to reach 95% steady-state current is less than 2s, indicating that H2O2 undergoes a rapid reduction process on the phosphorus molybdenum oxygen cluster crystal-CPE. In the linear range of 50-450μM, the current response of the phosphorus molybdenum oxygen cluster crystal-CPE shows a good linear relationship with the H2O2 concentration, and the linear regression equation is I H2O2 =0.085C H2O2 +10.778(R 2 =0.999), the sensitivity is 0.085μA·μM -1 The detection limit was calculated to be 3.52 μM (S / N=3).
[0049] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material, characterized in that: Its chemical formula is: H2(NH4)3[[C3N2H5][(P III O3)2Mo5O 15 ]·4H2O, crystallized in monoclinic system, C2y space group, the specific structure of the phosphorus molybdenum oxygen cluster crystal is described as follows: The phosphomolybdenum oxide cluster crystal consists of a [(P III O3)2Mo5O 15 ] 6- Polyanions, two [H] + , three [NH4] + , one [C3N2H5] + It consists of a cation and four crystal water molecules.
2. A method for preparing a three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material, characterized in that: The following steps are involved: Step 1: Take H3PO3 and (NH4)6Mo7O 24 4H2O was dissolved in 20ml water; Step 2: Adjust the pH value of the solution to 0.6 with hydrochloric acid; Step 3: heating the obtained solution to 60°C, and adding praseodymium chloride and imidazole to the hot solution; Step 4: The pH value of the solution was adjusted to 4.0 with aqueous ammonia, the solution was heated at 60°C for 30 minutes, the mixture was filtered and cooled to ambient temperature, and white block crystals were separated after 3 days.
3. A three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and a preparation method thereof according to claim 1, characterized in that: Step 1: Take H3PO3 and (NH4)6Mo7O 24 ·4H2O is dissolved in 20ml water, the amount of H3PO3 is 0.3g, 3.65mmol, (NH4)6Mo7O 24 The amount of 4H2O used is 1.235 g, 1.0 mmol.
4. The three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and the preparation method thereof according to claim 1, characterized in that: In the step 2, the molar concentration of hydrochloric acid in the process of adjusting the pH value of the solution to 0.6 with hydrochloric acid is 4 mol / L.
5. The three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and the preparation method thereof according to claim 1, characterized in that: The step three: heating the obtained solution to 60° C., and adding praseodymium chloride and imidazole to the hot solution, wherein the amount of praseodymium chloride used is 0.1 g, 0.695 mmol, and the amount of imidazole used is 0.1 g, 1.469 mmol.
6. The three-dimensional supramolecular structure phosphorus molybdenum oxygen cluster crystal material and the preparation method thereof according to claim 1, characterized in that: The step 4: adjusting the pH value of the solution to 4.0 with ammonia water, heating the solution at 60° C. for 30 minutes, filtering the mixture and cooling it to ambient temperature, and separating white block crystals after 3 days. The molar concentration of ammonia water in the process is 1 mol / L.
Citation Information
Cited By
Hexamethylenetetramine crystal material and preparation method thereof
CN119504768A
A hexamethylenetetramine crystal material and a preparation method thereof
CN119504768B