Anionic membrane containing heterogeneous dication applied to ECO2RR and preparation method thereof

By using a heterogeneous dicationic anion membrane in the carbon dioxide electroreduction reaction, combined with phenyl monomers and imidazolium functional groups, the problem of high product permeability and hydrogen evolution reaction of the Nafion membrane in the carbon dioxide electroreduction reaction was solved, achieving high efficiency. The effect of carbon dioxide electroreduction and manufacturing cost reduction.

CN118852702APending Publication Date: 2024-10-29JILIN ELECTRIC POWER RES INST LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410817501.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing Nafion series cation exchange membranes have problems with high product permeability and hydrogen evolution reaction in the carbon dioxide electroreduction reaction, resulting in low efficiency and high manufacturing costs.

Method used

A membrane containing heterogeneous dicationic anions is used, and a specific combination of phenyl monomers and imidazolium functional groups is used to prepare a membrane with good mechanical properties and high ion conductivity, which promotes ion transport and catalyzes the electroreduction of carbon dioxide.

Benefits of technology

It improves the carbon dioxide electroreduction efficiency, reduces the manufacturing cost of the membrane, enhances the alkali resistance and dimensional stability of the membrane, and significantly increases the ionic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852702A_ABST
    Figure CN118852702A_ABST
Patent Text Reader

Abstract

The invention discloses a heterogeneous dication-containing anion membrane applied to ECO2RR and a preparation method of the heterogeneous dication-containing anion membrane, and belongs to the technical field of anion exchange membranes. The heterogeneous dication-containing anion membrane is prepared by carrying out Friedel-Crafts hydroxyalkylation reaction on benzene derivatives containing electron donating groups, aldehyde benzene derivatives and aldehyde aliphatic hydrocarbon substances. The content of different types of functional ions in a polymer chain segment is adjusted by controlling the feeding proportion of monomers, and the dication functionalized anion exchange membrane containing quaternary ammonium functional groups and imidazolium functional groups is synthesized. The prepared membrane has good mechanical properties and ionic conductivity and has a certain promotion effect on electroreduction of carbon dioxide due to the fact that the dication structure can effectively promote transmission of ions, and the imidazolium functional group has an assistant catalysis function on electroreduction of carbon dioxide and can be applied to electroreduction of carbon dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anion exchange membranes, and in particular relates to a preparation process of an anion membrane containing heterogeneous dications used in ECO2RR. Background Art

[0002] With the rapid development of society and industrialization, the use of traditional fossil fuels such as coal, oil and natural gas has continued to increase, resulting in a rapid increase in the concentration of carbon dioxide in the environment, leading to a series of problems such as global warming, rising sea levels and energy depletion, which have become more serious. Although the increase in the carbon dioxide content in the atmosphere is the culprit for the rise in temperature, it itself is a convenient C1 raw material with extremely high energy value. Carbon dioxide electroreduction technology (eCO2RR) as an environmentally friendly reaction can not only reduce the carbon dioxide content in the atmosphere but also generate carbon monoxide, formic acid, methanol, ethylene and other substances for use as fuel, medicine and daily necessities. In this way, the economic cycle and energy renewableness of CO2 are realized, and the current severe environmental problems are solved, killing two birds with one stone. It has the advantages of high efficiency, sustainability, mild reaction conditions, scalability and diversity, and has become one of the effective ways to achieve artificial carbon cycle.

[0003] Compared with other thermal and photochemical reduction technologies, eCO2RR is a simple, low-cost and promising method that converts CO2 electrochemically into value-added chemicals such as formic acid. Formic acid is an important intermediate in chemical reactions and has important uses in many fields, such as fertilizers and pharmaceuticals, chemical raw materials, hydrogen storage and fuel cells. At present, most of the ion exchange membranes used in carbon dioxide electroreduction technologies are commercial Nafion series cation exchange membranes, but Nafion membranes have high permeability to products such as formic acid (CHOOH) and methanol (CH3OH) and good proton permeability, so that the products pass through the Nafion membrane to the anode and the protons pass through the Nafion membrane to the cathode for hydrogen evolution reaction, which greatly reduces the efficiency of eCO2RR. Therefore, the application of Nafion membranes in eCO2RR is limited. In order to solve the related defects of cation exchange membranes, anion exchange membranes have gradually appeared in the sight of many scholars, especially as an alternative membrane to cation exchange membranes in eCO2RR under alkaline conditions. Anion exchange membranes (AEMs) convert OH - The ions are transported from the cathode to the anode, which is in line with the direction of ion transport for carbon dioxide electroreduction, effectively inhibiting the occurrence of hydrogen evolution reaction and product permeation and reducing the manufacturing cost of the membrane. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a heterogeneous dicationic anion membrane used in ECO2RR and a preparation method thereof. The prepared membrane has good mechanical properties and ion conductivity and has a certain promoting effect on carbon dioxide electroreduction. This is because the structure of the dication can effectively promote the transmission of ions, and the imidazolium functional group has a catalytic function for the electroreduction of carbon dioxide, and can be used in carbon dioxide electroreduction.

[0005] The heterogeneous dicationic anion membrane used in ECO2RR is characterized by comprising the following repeating units:

[0006]

[0007] The Ar1 three-dimensional phenyl monomer is selected from the following structures:

[0008]

[0009] The Ar2 linear structure phenyl monomer is selected from the following structures:

[0010]

[0011] The R monomer is selected from the following structures:

[0012]

[0013] The n=0~1.

[0014] The preparation method of the heterogeneous dicationic anion membrane used in ECO2RR comprises the following steps:

[0015] Step 1, dissolving a linear phenyl monomer, an aldehyde aliphatic hydrocarbon monomer and a diketoindoline in dichloromethane, and controlling the ratio of two cations in the polymer by controlling the addition amount of the aldehyde aliphatic hydrocarbon monomer and the diketoindoline; slowly adding trifluoromethanesulfonic acid dropwise under an ice bath, and reacting for 6 hours to obtain a viscous solution; pouring the solution into a poor solvent for precipitation to precipitate the polymer main chain;

[0016] Step 2, crushing the main chain of the polymer, collecting the fragments by filtration, washing with a potassium carbonate solution, then washing three times with deionized water, and finally washing three times with anhydrous ethanol, and drying to obtain a copolymer;

[0017] Step 3, dissolving the copolymer in an organic solvent, adding potassium carbonate and methyl iodide to react, pouring the reaction mixture into a poor solvent for precipitation, washing until neutral, and drying the product in a vacuum drying oven to obtain a quaternized copolymer;

[0018] Step 4, dissolving the quaternized copolymer in an organic solvent, adding potassium carbonate and an ionizing agent to react, pouring the reaction mixture into a poor solvent for precipitation, washing to neutrality, and drying the product in a vacuum drying oven to obtain a copolymer containing a long side chain imidazolium;

[0019] Step 5, weighing the long side chain imidazolium copolymer and dissolving it in an organic solvent, filtering the solution through a 0.25-0.45 um polytetrafluoroethylene (PTFE) filter, casting and heating on glass to form a film, and obtaining a Br-type branched structure anion exchange membrane;

[0020] Step 6: peel off the Br-type heterogeneous dication functionalized anion exchange membrane from the glass plate, soak it in an alkaline solution, and then wash it with deionized water to obtain an OH-type heterogeneous dication functionalized anion exchange membrane.

[0021] The molar ratio of the linear structure phenyl monomer, the aldehyde aliphatic hydrocarbon monomer and the diketoindoline in step 1 is 8.5-9.5:3.5-5.5:3.5-5.5; the molar concentration of the diketoindoline in dichloromethane is 1-2 mol / L; the molar ratio of the diketoindoline to trifluoromethanesulfonic acid is 1:10-12; the poor solvents in steps 1, 3 and 4 are all water, methanol and ethanol.

[0022] In step 2, the concentration of the potassium carbonate solution is 1 to 3 M, the washing temperature is 30 to 60° C., and the washing time is 1 to 4 hours.

[0023] The organic solvents described in step three and step four are both N-methylpyrrolidone or dimethyl sulfoxide; the molar concentration of the copolymer in the organic solvent is 0.1-1 mol / L; the molar ratio of the copolymer to the ionizing agent is 1:1.5-2; the molar ratio of the polymer to potassium carbonate is 1:2-5; the reaction temperature in step three is 20-35°C and the time is 5-10h; the reaction temperature in step four is 80-100°C and the time is 5-10h.

[0024] In step 5, the organic solvent is N-methylpyrrolidone or dimethyl sulfoxide; the solubility of the quaternary ammonium copolymer in the solvent is 0.02-0.04 g / mL; the casting temperature is 50-100° C., and the casting time is 5-24 h.

[0025] Step 6: The OH-type heterogeneous double cation functionalized anion exchange membrane is stored in deionized water with nitrogen; the alkaline solution is potassium hydroxide or sodium hydroxide with a concentration of 0.5 to 2.0 M; the immersion temperature is 60 to 80° C. and the time is 1 to 24 hours.

[0026] Through the above-mentioned design scheme, the present invention can bring the following beneficial effects: the heterogeneous dicationic anion membrane used in the present invention in ECO2RR belongs to a polymer material without an aromatic ether skeleton, and the material has strong dimensional stability, high ionic conductivity, and good mechanical strength. The anion exchange membrane of the present invention overcomes the problem of poor chemical stability caused by ether bonds in the polymer main chain. The heterogeneous dicationic functional groups introduced in the present invention improve the microphase separation structure of the polymer, and at the same time, the imidazolium functional groups can effectively assist the electrochemical reduction of CO2. The membrane promotes the electrochemical reduction of CO2 while improving the ionic conductivity of the membrane.

[0027] Further beneficial effects of the present invention are:

[0028] (1) The membrane preparation process is simple. By using diketoindoline highly active reaction monomers, the reaction activity can be improved, the amount of catalyst used can be reduced, and the cost can be reduced;

[0029] (2) The present invention introduces a rigid phenyl structure to synthesize a polymer functionalized with quaternary ammonium and long side chain imidazolium double cations, which promotes the formation of ion clusters and hydrophilic-hydrophobic microphase separation, and significantly improves the conductivity of the membrane;

[0030] (3) The introduction of long side chain imidazolium functional groups can effectively assist the reduction of carbon dioxide gas and improve the efficiency of carbon dioxide electroreduction;

[0031] (4) The use of an ether-free main chain reduces the risk of hydroxide attack on the membrane, thereby enhancing the alkali resistance of the anion membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention is further described below with reference to the accompanying drawings and specific embodiments:

[0033] Figure 1 Schematic diagram of the synthesis route of Examples 1 to 3 of heterogeneous dicationic anion membranes used in ECO2RR according to the present invention.

[0034] Figure 2 It is a schematic diagram of the infrared spectrum of an embodiment of the present invention containing a heterogeneous dicationic anion membrane applied in ECO2RR.

[0035] Figure 3 Schematic diagram of thermal characterization of Examples 1 to 3 of the present invention containing heterogeneous dicationic anion membranes in ECO2RR.

[0036] Figure 4 Schematic diagram of water absorption at different temperatures of Examples 1 to 3 containing heterogeneous dicationic anion membranes used in ECO2RR according to the present invention.

[0037] Figure 5Schematic diagram of the dimensional change rate at different temperatures of Examples 1 to 3 containing heterogeneous dicationic anion membranes applied to ECO2RR of the present invention.

[0038] Figure 6 This is a schematic diagram of the conductivity of various ions at different temperatures in Example 1 of the present invention containing a heterogeneous dicationic anion membrane applied to ECO2RR.

[0039] Figure 7 Schematic diagram of the carbon dioxide electroreduction performance of Example 1 containing a heterogeneous dicationic anion membrane applied to ECO2RR of the present invention.

[0040] Figure 8 This is a performance diagram of the durability test of carbon dioxide electroreduction in Example 1 of the present invention containing a heterogeneous dicationic anion membrane applied to ECO2RR.

[0041] Fig. 9 Schematic diagram of the performance of carbon dioxide electroreduction in Example 2 of the present invention applied to ECO2RR containing a heterogeneous dicationic anion membrane.

[0042] Fig.10 This is a performance diagram of the durability test of carbon dioxide electroreduction in Example 2 of the present invention containing a heterogeneous dicationic anion membrane applied to ECO2RR.

[0043] Fig.11 Schematic diagram of the carbon dioxide electroreduction performance of Example 3 of the present invention containing a heterogeneous dicationic anion membrane applied to ECO2RR.

[0044] Fig.12 This is a performance diagram of the durability test of carbon dioxide electroreduction in Example 3 of the present invention containing a heterogeneous dicationic anion membrane applied to ECO2RR. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with implementation examples, but the implementation methods of the present invention are not limited thereto.

[0046] Embodiment 1:

[0047] 1. Prepare a polymer backbone with a cation ratio of 5:5. Pour p-terphenyl (4.19 g, 9 mmol), nitrogen methyl piperidone (0.51 g, 4.5 mmol), diketo indoline (0.66 g, 4.5 mmol) and dichloromethane (20 mL) into a 50 mL round-bottom flask equipped with a magnetic rod. Slowly drop trifluoromethanesulfonic acid (16.19 ml, 10 mmol) under an ice bath, react at 25 ° C for 6 hours, and the color of the solution changes from orange to dark red. Pour the viscous liquid into excess ethanol to precipitate a light yellow polymer backbone.

[0048] 2. The light yellow polymer main chain was crushed, the fragments were collected by filtration, washed with potassium carbonate solution (1M, 500 ml), then washed three times with deionized water, and finally washed three times with anhydrous ethanol, and dried to obtain a copolymer (PTPI).

[0049]

[0050] 3. Ionization of the copolymer: PTPI (3 g, 1 mmol) was dissolved in 75 mL of dimethyl sulfoxide solution under nitrogen atmosphere, potassium carbonate (2.11 g, 2 mmol) and ionizing agent (potassium iodide) (0.23 g, 1.5 mmol) were added to react, and heated to 80°C and stirred for 9 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain a quaternized copolymer (QPTPI);

[0051] 4. Copolymer grafted with imidazolium long side chain, QPTPI (3g, 1mmol) was dissolved in 75mL dimethyl sulfoxide solution under nitrogen environment, potassium carbonate (2.11g, 2mmol) and ionizing agent (3-(6-bromohexyl)-1-methyl-1H-imidazol-3-imidazolium) (1.86g, 1.5mmol) were added to react, heated to 100°C and stirred for 12 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain an imidazolium grafted copolymer (QPTPI-MIM);

[0052] 5. Weigh 0.22g of the prepared quaternary ammonium copolymer (QPTPI-MIM) and dissolve it in 8ml of dimethyl sulfoxide solution. Filter the polymer solution through a 0.25-0.45um polytetrafluoroethylene (PTFE) filter and heat it on a glass plate to form a film. The casting reaction temperature is 70°C and the casting time is 12h. - Heterogeneous dual cation functionalized anion exchange membrane.

[0053] 6. The Br-type heterogeneous dication functionalized anion exchange membrane was peeled off from the glass plate, immersed in a 1M potassium hydroxide solution at 60°C for 12 hours, and then washed with deionized water to obtain an OH-type heterogeneous dication functionalized anion exchange membrane. To avoid CO2 contamination and carbonate formation, the membrane was immersed in deionized water with nitrogen for storage.

[0054]

[0055] In the anion exchange membrane obtained in Example 1, the three-dimensional structure phenyl monomer Ar1 is selected from Formula 101, the linear structure phenyl monomer Ar2 is selected from Formula 203, and the R monomer is selected from Formula 301;

[0056] Embodiment 2:

[0057] 1. Prepare a polymer backbone with a cation ratio of 4:6. Pour p-diphenylethane (3.57 g, 9.5 mmol), nitrogen methyl piperidone (0.43 g, 3.8 mmol), diketoindoline (0.84 g, 5.7 mmol) and dichloromethane (12 mL) into a 50 mL round-bottom flask equipped with a magnetic rod. Slowly drop trifluoromethanesulfonic acid (15.78 ml, 11 mmol) under an ice bath, react at 25 ° C for 12 hours, and the color of the solution changes from orange to dark red. Pour the viscous liquid into excess ethanol to precipitate a light yellow polymer backbone.

[0058] 2. The light yellow polymer main chain was crushed, the fragments were collected by filtration, washed with potassium carbonate solution (1M, 500 ml), then washed three times with deionized water, and finally washed three times with anhydrous ethanol, and dried to obtain a copolymer (PDPI).

[0059]

[0060] 3. Ionization of the copolymer: PDPI (3 g, 1 mmol) was dissolved in 75 mL of dimethyl sulfoxide solution under nitrogen atmosphere, potassium carbonate (2.11 g, 2 mmol) and ionizing agent (potassium iodide) (0.23 g, 1.5 mmol) were added to react, and the mixture was heated to 80°C and stirred for 9 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain a quaternized copolymer (QPDPI);

[0061] 4. Copolymer grafted with imidazolium long side chain, QPDPI (3g, 1mmol) was dissolved in 75mL dimethyl sulfoxide solution under nitrogen environment, potassium carbonate (2.11g, 2mmol) and ionizing agent (3-(6-bromohexyl)-1-methyl-1H-imidazol-3-imidazolium) (1.86g, 1.5mmol) were added for reaction, heated to 100°C and stirred for 12 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain an imidazolium grafted copolymer (QPDPI-MIM);

[0062] 5. Weigh 0.22g of the prepared quaternary ammonium copolymer (QPDPI-MIM) and dissolve it in 8ml of dimethyl sulfoxide solution. The polymer solution is filtered through a 0.25-0.45um polytetrafluoroethylene (PTFE) filter and heated to form a film by casting on a glass plate. The casting reaction temperature is 70°C and the casting time is 12h. The Br-type heterogeneous double cation functionalized anion exchange membrane is obtained.

[0063] 6. The Br-type heterogeneous dication functionalized anion exchange membrane was peeled off from the glass plate, immersed in a 1M potassium hydroxide solution at 60°C for 12 hours, and then washed with deionized water to obtain an OH-type heterogeneous dication functionalized anion exchange membrane. To avoid CO2 contamination and carbonate formation, the membrane was immersed in deionized water with nitrogen for storage.

[0064]

[0065] In the anion exchange membrane obtained in Example 2, the three-dimensional structure phenyl monomer of Ar1 is selected from Formula 104, the linear structure phenyl monomer of Ar2 is selected from Formula 203, and the R monomer is selected from Formula 301;

[0066] Embodiment 3:

[0067] 1. Prepare a polymer backbone with a cation ratio of 2:8. Pour p-terphenyl (3.19 g, 8.5 mmol), nitrogen methyl piperidone (0.19 g, 1.5 mmol), diketo indoline (1.1 g, 6.8 mmol) and dichloromethane (10.60 ml) into a 50 mL round-bottom flask equipped with a magnetic rod. Slowly drop trifluoromethanesulfonic acid (20.35 ml, 12 mmol) under an ice bath, react at 25 ° C for 6 hours, and the color of the solution changes from orange to dark red. Pour the viscous liquid into excess ethanol to precipitate a light yellow polymer backbone.

[0068] 2. The light yellow polymer main chain was crushed, the fragments were collected by filtration, washed with potassium carbonate solution (1M, 500 ml), then washed three times with deionized water, and finally washed three times with anhydrous ethanol, and dried to obtain a copolymer (PTPI).

[0069]

[0070] 3. Ionization of the copolymer: PTPI (3 g, 1 mmol) was dissolved in 75 mL of dimethyl sulfoxide solution under nitrogen atmosphere, potassium carbonate (2.11 g, 2 mmol) and ionizing agent (potassium iodide) (0.28 g, 2 mmol) were added to react, and the mixture was heated to 80°C and stirred for 9 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain a quaternized copolymer (QPTPI);

[0071] 4. Copolymer grafted with imidazolium long side chain, QPTPI (3g, 1mmol) was dissolved in 75mL dimethyl sulfoxide solution under nitrogen environment, potassium carbonate (2.11g, 2mmol) and ionizing agent (3-(6-bromohexyl)-1-methyl-1H-imidazol-3-imidazolium) (3.98g, 2mmol) were added to react, heated to 100°C and stirred for 12 hours. The reaction mixture was poured into deionized water for precipitation and washed to neutrality, and the product was placed in a vacuum drying oven for drying to obtain an imidazolium grafted copolymer (QPTPI-TMIM);

[0072] 5. Weigh 0.22g of the prepared quaternary ammonium copolymer (QPTPI-TMIM) and dissolve it in 8ml of dimethyl sulfoxide solution. Filter the polymer solution through a 0.25-0.45um polytetrafluoroethylene (PTFE) filter and heat it on a glass plate to form a film. The casting reaction temperature is 70°C and the casting time is 12h. - Heterogeneous dual cation functionalized anion exchange membrane.

[0073] 6. The Br-type heterogeneous dication functionalized anion exchange membrane was peeled off from the glass plate, immersed in a 1M potassium hydroxide solution at 60°C for 12 hours, and then washed with deionized water to obtain an OH-type heterogeneous dication functionalized anion exchange membrane. To avoid CO2 contamination and carbonate formation, the membrane was immersed in deionized water with nitrogen for storage.

[0074]

[0075] In the anion exchange membrane obtained in Example 2, the three-dimensional structure phenyl monomer Ar1 is selected from Formula 101, the linear structure phenyl monomer Ar2 is selected from Formula 203, and the R monomer is selected from Formula 302;

[0076] Taking the heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR as described in Examples 1 to 3 as an example, Figure 1 The synthetic route of the heterogeneous dication-containing anion membrane (QPTPI-MIM) used in ECO2RR is presented.

[0077] The heterogeneous dication-containing anion membrane (QPTPI-MIM) used in ECO2RR as described in Example 1 was structurally characterized using Fourier transform infrared spectroscopy to confirm the synthesis of the target compound.

[0078] The heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR described in Example 1 was used as a sample. The dried sample was heated from 80°C to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere to obtain the degradation curve of the polymer with increasing temperature. Figure 3 It can be concluded that the polymer does not decompose within 200°C and is suitable for carbon dioxide electroreduction equipment.

[0079] The heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR described in Examples 1 to 3 was used as a sample. Figure 4 and Figure 5 As shown in the figure, water absorption rate (WU) and swelling rate (SR) tests were carried out as follows: the dried film samples were immersed in deionized water at different temperatures for 24 h to allow the film to fully absorb water to saturation, and the mass and length of the film before and after soaking in water were measured, which were recorded as WU, WU and SR, respectively. dry ,W wet and L dry ,L wet The calculation method is as follows:

[0080]

[0081] The conductivity test was carried out using the heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR as described in Examples 1 to 3; Figure 7 , the conductivity of the heterogeneous double cation functionalized ion exchange membrane at 30℃-80℃ was tested by electrochemical impedance spectroscopy (EIS), and the CHI760e electrochemical workstation was used for measurement. The test frequency was 1MHz-0.01Hz. In the experiment, the membrane was cut into a size of 10mm×50mm, and the membrane was placed in a polytetrafluoroethylene fixture. The test was carried out under 100% humidity conditions, and finally the ionic conductivity σ of the sample was calculated according to the formula; σ=L / (wdR) In the formula, L is the length of the membrane between the electrodes (cm), w is the width of the membrane (cm), d is the thickness of the membrane (cm), and R is the measured resistance of the membrane (Ω);

[0082] Taking the heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR as described in Example 1 as an example, the performance test of carbon dioxide electroreduction of formic acid was carried out; Figure 7 It shows that a current density of 622.4V can be achieved at 3.6V. During the test, the assembled battery was kept at 60℃, and 80sccm of CO2 gas was provided to the cathode. During operation, the cathode gas flow was passed to the cathode under the conditions of 100% relative humidity and 60℃ heating. The anode was passed with 1mol L heated to 60℃ at a flow rate of 15mL / min. -1 KOH solution.

[0083] The durability test of carbon dioxide electroreduction of formic acid was carried out using the heterogeneous dicationic anion membrane (QPTPI-MIM) used in ECO2RR as described in Example 1 as a sample; Figure 8 Display, at 100mA cm -2 The battery was able to operate stably at around 2.7V for more than 14 hours at a current density of 2.7V. During the test, the assembled battery was kept at 60°C, and 40sccm of CO2 gas was provided to the cathode. During operation, the cathode gas flow was passed to the cathode at a relative humidity of 100% and heated at 60°C. The anode was passed with 1 mol L heated to 60°C at a flow rate of 7mL / min. -1 KOH solution.

[0084] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. Application to ECO 2 RR contains heterogeneous dicationic anion membrane, Its characteristics are: The following repeating units are included:

2. The method for applying to ECO according to claim 1 2 RR contains heterogeneous dicationic anion membrane, Its characteristics are: The Ar 1 The three-dimensional phenyl monomer is selected from the following structures:

3. The method for applying to ECO according to claim 1 2 RR contains heterogeneous dicationic anion membrane, Its characteristics are: The Ar 2 The linear phenyl monomer is selected from the following structures:

4. The method for applying to ECO according to claim 1 2 RR contains heterogeneous dicationic anion membrane, Its characteristics are: The R monomer is selected from the following structures: The n=0~1.

5. Application to ECO 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: Preparation of the method for use in ECO as claimed in claim 1 2 The RR contains a heterogeneous dicationic anion membrane, comprising the following steps: Step 1, dissolving a linear phenyl monomer, an aldehyde aliphatic hydrocarbon monomer and a diketoindoline in dichloromethane, and controlling the ratio of two cations in the polymer by controlling the addition amount of the aldehyde aliphatic hydrocarbon monomer and the diketoindoline; slowly adding trifluoromethanesulfonic acid dropwise under an ice bath, and reacting for 6 hours to obtain a viscous solution; pouring the solution into a poor solvent for precipitation to precipitate the polymer main chain; Step 2, crushing the main chain of the polymer, collecting the fragments by filtration, washing with a potassium carbonate solution, then washing three times with deionized water, and finally washing three times with anhydrous ethanol, and drying to obtain a copolymer; Step 3, dissolving the copolymer in an organic solvent, adding potassium carbonate and methyl iodide to react, pouring the reaction mixture into a poor solvent for precipitation, washing until neutral, and drying the product in a vacuum drying oven to obtain a quaternized copolymer; Step 4, dissolving the quaternized copolymer in an organic solvent, adding potassium carbonate and an ionizing agent to react, pouring the reaction mixture into a poor solvent for precipitation, washing to neutrality, and drying the product in a vacuum drying oven to obtain a copolymer containing a long side chain imidazolium; Step 5, weighing the long side chain imidazolium copolymer and dissolving it in an organic solvent, filtering the solution through a 0.25-0.45 um polytetrafluoroethylene (PTFE) filter, casting and heating on glass to form a film, and obtaining a Br-type branched structure anion exchange membrane; Step 6: peel off the Br-type heterogeneous dication functionalized anion exchange membrane from the glass plate, soak it in an alkaline solution, and then wash it with deionized water to obtain an OH-type heterogeneous dication functionalized anion exchange membrane.

6. The method for applying to ECO according to claim 5 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: Steps 1. The molar ratio of the linear structure phenyl monomer, the aldehyde aliphatic hydrocarbon monomer and the diketoindoline is 8.5-9.5:3.5-5.5:3.5-5.5; the molar concentration of the diketoindoline in dichloromethane is 1-2 mol / L; the molar ratio of the diketoindoline to trifluoromethanesulfonic acid is 1:10-12; the poor solvents in step 1, step 3 and step 4 are all water, methanol and ethanol.

7. The method for applying to ECO according to claim 5 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: In step 2, the concentration of the potassium carbonate solution is 1 to 3 M, the washing temperature is 30 to 60° C., and the washing time is 1 to 4 hours.

8. The method for applying to ECO according to claim 5 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: The organic solvents described in step three and step four are both N-methylpyrrolidone or dimethyl sulfoxide; the molar concentration of the copolymer in the organic solvent is 0.1-1 mol / L; the molar ratio of the copolymer to the ionizing agent is 1:1.5-2; the molar ratio of the polymer to potassium carbonate is 1:2-5; the reaction temperature in step three is 20-35°C and the time is 5-10h; the reaction temperature in step four is 80-100°C and the time is 5-10h.

9. The method for applying to ECO according to claim 5 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: In step 5, the organic solvent is N-methylpyrrolidone or dimethyl sulfoxide; the solubility of the quaternary ammonium copolymer in the solvent is 0.02-0.04 g / mL; the casting temperature is 50-100° C., and the casting time is 5-24 h.

10. The method for applying to ECO according to claim 5 2 Preparation method of heterogeneous dicationic anion membrane in RR, Its characteristics are: Step 6: The OH-type heterogeneous double cation functionalized anion exchange membrane is stored in deionized water with nitrogen; the alkaline solution is potassium hydroxide or sodium hydroxide with a concentration of 0.5 to 2.0 M; the immersion temperature is 60 to 80° C. and the time is 1 to 24 hours.