High-conductivity carbon-coated slurry for battery foil and use method of high-conductivity carbon-coated slurry

By using nano-silver wrapped graphene compounded with carbon nanotubes and an optimized binder combination, the problem of insufficient conductivity of the existing carbon coating slurry is solved, and a coating with high conductivity and stability is achieved, which is suitable for lithium battery foils.

CN118852918APending Publication Date: 2024-10-29JIANGSU DINGSHENG NEW MATERIAL JOINT STOCK CO LTD

Patent Information

Application Number
CN202410900357.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing carbon coating slurry has insufficient conductivity and insufficient binder performance, making it difficult to meet the conductivity and electrochemical stability requirements of lithium battery foils.

Method used

Using nano-silver wrapped graphene compounded with carbon nanotubes as the conductive material, combined with high molecular weight polyvinylidene fluoride, acrylate copolymer and sodium silicate as the binder, through ultrasonic dispersion and staged drying and curing processes to form a highly conductive Sexual coating.

Benefits of technology

It significantly improves the conductive performance and stability of carbon-coated slurry, improves the mechanical strength, heat resistance and adhesion of the coating, and forms a uniform and dense conductive network.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides high-conductivity carbon-coated slurry as well as a preparation method and a use method thereof. The high-conductivity carbon-coated slurry is applicable to production of battery foils. The carbon coating slurry is composed of a conductive material, a binder A, a binder B, an inorganic binder and a solvent. The conductive material adopts nano-silver-coated graphene compounded carbon nanotubes, so that the conductivity is remarkably improved. The binder A is polyvinylidene fluoride with high molecular weight and provides excellent chemical stability and heat resistance; the binder B is an acrylate copolymer and has good adhesion performance and flexibility; the inorganic binder sodium silicate improves the heat resistance of the coating and the stability of the conductivity. Through a staged drying and curing process, the slurry forms a uniform and compact conductive network, and the mechanical strength and conductivity of the coating are enhanced. The carbon-coated slurry is excellent in conductivity, mechanical strength, adhesive force and durability, the performance of the battery foil is remarkably improved, the service life of the battery foil is remarkably prolonged, and the requirement of a high-performance battery is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a field of preparation of carbon coating slurry, and more particularly relates to a high-conductivity carbon coating slurry for battery foil and a use method thereof. Background Art

[0002] With the continuous growth of global energy demand and the enhancement of environmental protection awareness, new energy technology, especially lithium battery technology, has developed rapidly. Lithium batteries are widely used in electric vehicles, mobile devices and energy storage systems due to their high energy density, long cycle life and good safety performance. In the manufacturing process of lithium batteries, the selection and processing of battery foil materials have a crucial impact on the comprehensive performance of the battery.

[0003] Battery foil is usually made of aluminum foil and serves as the current collector for the positive and negative electrodes of lithium batteries. In order to improve the conductivity and electrochemical stability of the battery, a conductive coating needs to be coated on the surface of the battery foil. Traditional coating materials usually include carbon materials and polymer binders. However, the conductive paste used in the prior art has some shortcomings, mainly manifested in that the conductivity of the carbon-coated paste is not enough to meet current requirements and the binder of the carbon-coated paste is not enough, so further improvements are needed. Summary of the invention

[0004] In order to solve the problems existing in the prior art, a highly conductive carbon-coated slurry for battery foil and a method for using the same are provided. The specific scheme is as follows:

[0005] A highly conductive carbon-coated slurry for battery foil, applied to battery foil, the carbon-coated slurry comprising the following components:

[0006] Conductive material: nano-silver wrapped graphene compounded with carbon nanotubes;

[0007] Binder A: polyvinylidene fluoride;

[0008] Binder B: acrylate copolymer;

[0009] Inorganic binder: sodium silicate;

[0010] Solvent: dimethyl sulfoxide;

[0011] The modulus of SiO and Na2O in the sodium silicate is 3.0 to 3.5.

[0012] Furthermore, the preparation method of nanosilver-wrapped graphene-compounded carbon nanotubes comprises the following steps:

[0013] S1, preparing nano silver particles;

[0014] S2. Preparation of nanosilver-wrapped graphene:

[0015] S201, dispersing graphene: taking graphene powder, adding it into dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse it for 30 minutes;

[0016] S202, mixing nanosilver and graphene: adding dry nanosilver powder to the graphene dispersion, and continuing ultrasonic stirring for 1 hour to ensure that the nanosilver is evenly distributed on the graphene surface;

[0017] S3, graphene surface coated with carbon nanotubes:

[0018] S301, dispersing carbon nanotubes: taking carbon nanotubes, adding them into dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse them for 30 minutes;

[0019] S302, mixing and coating: slowly adding the dispersed carbon nanotubes into the dispersion of nanosilver-wrapped graphene and stirring evenly; stirring at room temperature for 3 hours using a stirrer to allow the carbon nanotubes to be evenly coated on the composite structure of nanosilver and graphene.

[0020] Furthermore, S1 preparing the nano silver particles further comprises the following steps:

[0021] S101: Prepare silver nitrate solution and sodium hydroxide solution;

[0022] S102, solution preparation: add silver nitrate solution to a reaction flask, add sodium hydroxide solution dropwise under stirring to make the solution weakly alkaline; add glucose solution, continue stirring and reacting for 1 hour, and control the reaction temperature at 60°C;

[0023] S103, washing and drying: after the reaction is completed, the product is repeatedly washed by centrifugation with deionized water until the washing liquid is colorless; the washed nanosilver particles are vacuum dried at 60° C. for 12 hours to obtain dry nanosilver powder.

[0024] Furthermore, the molecular weight of polyvinylidene fluoride is 400,000 to 700,000 g / mol.

[0025] Furthermore, the molecular weight of the acrylic ester copolymer is 100,000 to 300,000 g / mol.

[0026] A method for using a highly conductive carbon-coated slurry for battery foil comprises the following steps:

[0027] S1. Substrate preparation: Aluminum foil is selected as the substrate and pre-treated;

[0028] S2, preparation of carbon coating slurry: weigh nanosilver-wrapped graphene composite carbon nanotubes, and disperse them in dimethyl sulfoxide, and use an ultrasonic processor to ultrasonically disperse for 30 minutes; add polyvinylidene fluoride and acrylate copolymer according to the mass ratio, and stir evenly; add an appropriate amount of sodium silicate, and continue stirring for 30 minutes until the slurry is uniform;

[0029] S3, coating: evenly coating the prepared carbon coating slurry on the surface of the substrate; the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense;

[0030] S4, drying and curing: placing the coated substrate into an oven for stage-by-stage drying and curing.

[0031] Furthermore, the parameters of the staged drying and curing in S4 are: drying the coated substrate in stages at 60°C, 80°C and 100°C, with a drying time of 30 minutes in each stage; and finally drying at 120°C for 2 hours to ensure that the coating is completely cured.

[0032] Beneficial effects:

[0033] The present invention provides a highly conductive carbon-coated slurry for battery foil and a method for using the same, which specifically includes the following advantages:

[0034] (1) The conductive material is nanosilver wrapped in graphene and compounded with carbon nanotubes, which significantly improves the conductivity of the carbon-coated slurry. Nanosilver has excellent conductivity, and wrapping it on graphene can improve the conductivity of graphene. At the same time, carbon nanotubes further enhance the stability and continuity of the conductive network. This composite structure makes the conductive material perform well in terms of high conductivity and stability.

[0035] (2) The composition of the binder in the slurry components was optimized, and a combination of binder A, binder B and inorganic binder was used, wherein binder A polyvinylidene fluoride: high molecular weight polyvinylidene fluoride (molecular weight 400000-700000 g / mol) was used as a binder, which has good chemical stability and heat resistance, and can effectively enhance the mechanical strength and durability of the coating; binder B acrylate copolymer: acrylate copolymer with a molecular weight of 100000-300000 g / mol was selected, which has excellent adhesion and flexibility, and helps to improve the adhesion and toughness of the coating. Inorganic binder sodium silicate: sodium silicate (modulus 3.0-3.5) is used as an inorganic binder, which has high temperature stability and good adhesion, and can improve the heat resistance and conductivity stability of the coating.

[0036] (3) When using carbon coating slurry, the staged drying and curing process can better control the drying process of the slurry and avoid cracks and uneven shrinkage caused by rapid drying. After initial low-temperature drying, high-temperature curing helps to form a uniform and dense conductive network and improve the mechanical strength and conductive properties of the coating. DETAILED DESCRIPTION

[0037] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0038] Embodiment 1:

[0039] A method for preparing a highly conductive carbon-coated slurry for battery foil comprises the following steps:

[0040] Preparation of conductive materials:

[0041] Step S1: preparing nano silver particles:

[0042] Prepare silver nitrate solution and sodium hydroxide solution.

[0043] A 0.1 M silver nitrate solution was added to the reaction flask, and a 0.1 M sodium hydroxide solution was added dropwise under stirring to make the solution weakly alkaline.

[0044] Add 0.05 M glucose solution, continue stirring and react for 1 hour, and control the reaction temperature at 60°C.

[0045] After the reaction is completed, the product is repeatedly centrifuged and washed with deionized water until the washing liquid is colorless; the washed nanosilver particles are vacuum dried at 60° C. for 12 hours to obtain dry nanosilver powder.

[0046] Step S2: preparing nanosilver-wrapped graphene:

[0047] Step S201: dispersing graphene: taking 1 g of graphene powder, adding it into 100 mL of dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse it for 30 minutes.

[0048] Step S202: Mixing nanosilver and graphene: Add 1 g of dry nanosilver powder into the graphene dispersion, and continue ultrasonic stirring for 1 hour to ensure that the nanosilver is evenly distributed on the graphene surface.

[0049] Step S3: coating graphene surface with carbon nanotubes:

[0050] Step S301: Dispersing carbon nanotubes: 1 g of carbon nanotubes are added into 100 mL of dimethyl sulfoxide, and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0051] Step S302: Mixing and coating: slowly adding the dispersed carbon nanotubes into the dispersion of nanosilver-wrapped graphene and stirring evenly; stirring at room temperature for 3 hours using a stirrer to allow the carbon nanotubes to be evenly coated on the composite structure of nanosilver and graphene.

[0052] Preparation of carbon coating slurry:

[0053] The prepared nanosilver-wrapped graphene composite carbon nanotubes were dispersed in 100 mL of dimethyl sulfoxide and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0054] Add 1 g of polyvinylidene fluoride (molecular weight 400,000-700,000 g / mol) and 1 g of acrylate copolymer (molecular weight 100,000-300,000 g / mol) according to the mass ratio and stir evenly.

[0055] Add 0.5 g of sodium silicate and continue stirring for 30 minutes until the slurry is uniform.

[0056] Coating and curing:

[0057] The prepared carbon coating slurry is evenly coated on the surface of the aluminum foil substrate, and the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense.

[0058] The coated substrate was dried in stages at 60°C, 80°C and 100°C, with each stage drying time being 30 minutes; finally, it was dried at 120°C for 2 hours to ensure that the coating was completely cured.

[0059] Embodiment 2:

[0060] A method for preparing a highly conductive carbon-coated slurry for battery foil comprises the following steps:

[0061] Preparation of conductive materials:

[0062] Step S1: preparing nano silver particles:

[0063] Prepare 0.1 M silver nitrate solution and 0.1 M sodium hydroxide solution.

[0064] Under stirring, add sodium hydroxide solution dropwise to make the solution weakly alkaline.

[0065] Add 0.05 M glucose solution, continue stirring and react for 1 hour, and control the reaction temperature at 60°C.

[0066] After the reaction is completed, the product is repeatedly centrifuged and washed with deionized water until the washing liquid is colorless; the washed nanosilver particles are vacuum dried at 60° C. for 12 hours to obtain dry nanosilver powder.

[0067] Step S2: preparing nanosilver-wrapped graphene:

[0068] Step S201: Dispersing graphene: 1.5 g of graphene powder is added into 150 mL of dimethyl sulfoxide, and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0069] Step S202: Mixing nanosilver and graphene: Add 1.5 g of dry nanosilver powder into the graphene dispersion, and continue ultrasonic stirring for 1 hour to ensure that the nanosilver is evenly distributed on the graphene surface.

[0070] Step S3: coating graphene surface with carbon nanotubes:

[0071] Step S301: Dispersing carbon nanotubes: 1.5 g of carbon nanotubes are added into 150 mL of dimethyl sulfoxide, and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0072] Step S302: Mixing and coating: slowly adding the dispersed carbon nanotubes into the dispersion of nanosilver-wrapped graphene and stirring evenly; stirring at room temperature for 3 hours using a stirrer to allow the carbon nanotubes to be evenly coated on the composite structure of nanosilver and graphene.

[0073] Preparation of carbon coating slurry:

[0074] The prepared nanosilver-wrapped graphene composite carbon nanotubes were dispersed in 150 mL of dimethyl sulfoxide and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0075] 1.5 g of polyvinylidene fluoride (molecular weight 400,000-700,000 g / mol) and 1.5 g of acrylate copolymer (molecular weight 100,000-300,000 g / mol) were added according to the mass ratio and stirred evenly.

[0076] Add 0.75 g of sodium silicate and continue stirring for 30 minutes until the slurry is uniform.

[0077] Coating and curing:

[0078] The prepared carbon coating slurry is evenly coated on the surface of the aluminum foil substrate, and the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense.

[0079] The coated substrate was dried in stages at 60°C, 80°C and 100°C, with each stage drying time being 30 minutes; finally, it was dried at 120°C for 2 hours to ensure that the coating was completely cured.

[0080] Embodiment 3:

[0081] Preparation method of carbon coating slurry

[0082] Preparation of conductive materials:

[0083] Step S1: preparing nano silver particles:

[0084] Prepare 0.1 M silver nitrate solution and 0.1 M sodium hydroxide solution.

[0085] Under stirring, add sodium hydroxide solution dropwise to make the solution weakly alkaline.

[0086] Add 0.05 M glucose solution, continue stirring and react for 1 hour, and control the reaction temperature at 60°C.

[0087] After the reaction is completed, the product is repeatedly centrifuged and washed with deionized water until the washing liquid is colorless; the washed nanosilver particles are vacuum dried at 60° C. for 12 hours to obtain dry nanosilver powder.

[0088] Step S2: preparing nanosilver-wrapped graphene:

[0089] Step S201: dispersing graphene: taking 2 g of graphene powder, adding it into 200 mL of dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse it for 30 minutes.

[0090] Step S202: Mixing nanosilver and graphene: Add 2 g of dry nanosilver powder into the graphene dispersion, and continue ultrasonic stirring for 1 hour to ensure that the nanosilver is evenly distributed on the graphene surface.

[0091] Step S3: coating graphene surface with carbon nanotubes:

[0092] Step S301: dispersing carbon nanotubes: taking 2 g of carbon nanotubes, adding them into 200 mL of dimethyl sulfoxide, and using an ultrasonic processor to disperse them for 30 minutes.

[0093] Step S302: Mixing and coating: slowly adding the dispersed carbon nanotubes into the dispersion of nanosilver-wrapped graphene and stirring evenly; stirring at room temperature for 3 hours using a stirrer to allow the carbon nanotubes to be evenly coated on the composite structure of nanosilver and graphene.

[0094] Preparation of carbon coating slurry:

[0095] The prepared nanosilver-wrapped graphene composite carbon nanotubes were dispersed in 200 mL of dimethyl sulfoxide and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0096] Add 2 g of polyvinylidene fluoride (molecular weight 400000-700000 g / mol) and 2 g of acrylate copolymer (molecular weight 100000-300000 g / mol) according to the mass ratio and stir evenly.

[0097] Add 1 g of sodium silicate and continue stirring for 30 minutes until the slurry is uniform.

[0098] Coating and curing:

[0099] The prepared carbon coating slurry is evenly coated on the surface of the aluminum foil substrate, and the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense.

[0100] The coated substrate was dried in stages at 60°C, 80°C and 100°C, with each stage drying time of 30 minutes; finally dried at 120°C for 2 hours to ensure that the coating was completely cured. The carbon nanotubes were evenly coated in the dispersion of graphene; stirred at room temperature for 3 hours using a stirrer to make the carbon nanotubes evenly coated on the composite structure of nanosilver and graphene.

[0101] Preparation of carbon coating slurry:

[0102] The prepared nanosilver-wrapped graphene composite carbon nanotubes were dispersed in 200 mL of dimethyl sulfoxide and ultrasonically dispersed for 30 minutes using an ultrasonic processor.

[0103] Add 2 g of polyvinylidene fluoride (molecular weight 400000-700000 g / mol) and 2 g of acrylate copolymer (molecular weight 100000-300000 g / mol) according to the mass ratio and stir evenly.

[0104] Add 1 g of sodium silicate and continue stirring for 30 minutes until the slurry is uniform.

[0105] Coating and curing:

[0106] The prepared carbon coating slurry is evenly coated on the surface of the aluminum foil substrate, and the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense.

[0107] The coated substrate was dried in stages at 60°C, 80°C and 100°C, with each stage drying time being 30 minutes; finally, it was dried at 120°C for 2 hours to ensure that the coating was completely cured.

[0108] Comparative Example:

[0109] The carbon-coated slurry is prepared by conventional methods.

[0110] The carbon-coated slurries obtained in Examples 1 to 3 and the comparative example were tested for electrical conductivity, and the test results are as follows:

[0111] Example 1 Example 2 Example 3 Comparative Example Surface resistivity 8.5 7.8 7.2 15 Volume resistivity 0.002 0.0018 0.0016 0.005

[0112] The carbon-coated slurries prepared in Examples 1 to 3 have significantly lower surface resistivity and volume resistivity than those in the comparative example, indicating that the conductive properties of the carbon-coated slurries can be greatly improved by the preparation method of nanosilver-wrapped graphene-compounded carbon nanotubes and the optimized slurry formula.

[0113] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly conductive carbon-coated slurry for battery foil, applied to battery foil, characterized in that: The carbon coating slurry comprises the following components: Conductive material: nano-silver wrapped graphene compounded with carbon nanotubes; Binder A: polyvinylidene fluoride; Binder B: acrylate copolymer; Inorganic binder: sodium silicate; Solvent: dimethyl sulfoxide; The modulus of SiO and Na2O in the sodium silicate is 3.0 to 3.

5.

2. The highly conductive carbon-coated slurry for battery foil according to claim 1, characterized in that: The preparation method of nano-silver wrapped graphene composite carbon nanotubes comprises the following steps: S1, preparing nano silver particles; S2. Preparation of nanosilver-wrapped graphene: S201, dispersing graphene: taking graphene powder, adding it into dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse it for 30 minutes; S202, mixing nanosilver and graphene: adding dry nanosilver powder to the graphene dispersion, and continuing ultrasonic stirring for 1 hour to ensure that the nanosilver is evenly distributed on the graphene surface; S3, graphene surface coated with carbon nanotubes: S301, dispersing carbon nanotubes: taking carbon nanotubes, adding them into dimethyl sulfoxide, and using an ultrasonic processor to ultrasonically disperse them for 30 minutes; S302, mixing and coating: slowly adding the dispersed carbon nanotubes into the dispersion of nanosilver-wrapped graphene and stirring evenly; stirring at room temperature for 3 hours using a stirrer to allow the carbon nanotubes to be evenly coated on the composite structure of nanosilver and graphene.

3. The highly conductive carbon-coated slurry for battery foil according to claim 2, characterized in that: S1 preparation of nano silver particles also includes the following steps: S101: Prepare silver nitrate solution and sodium hydroxide solution; S102, solution preparation: add silver nitrate solution to a reaction flask, add sodium hydroxide solution dropwise under stirring to make the solution weakly alkaline; add glucose solution, continue stirring and reacting for 1 hour, and control the reaction temperature at 60°C; S103, washing and drying: after the reaction is completed, the product is repeatedly washed by centrifugation with deionized water until the washing liquid is colorless; the washed nanosilver particles are vacuum dried at 60° C. for 12 hours to obtain dry nanosilver powder.

4. The highly conductive carbon-coated slurry for battery foil according to claim 1, characterized in that: The molecular weight of polyvinylidene fluoride is 400,000 to 700,000 g / mol.

5. The highly conductive carbon-coated slurry for battery foil according to claim 1, characterized in that: The molecular weight of the acrylic ester copolymer is 100,000 to 300,000 g / mol.

6. A method for using a highly conductive carbon-coated slurry for battery foil, characterized in that: The following steps are involved: S1. Substrate preparation: Aluminum foil is selected as the substrate and pre-treated; S2, preparation of carbon coating slurry: weigh nanosilver-wrapped graphene composite carbon nanotubes, and disperse them in dimethyl sulfoxide, and use an ultrasonic processor to ultrasonically disperse for 30 minutes; add polyvinylidene fluoride and acrylate copolymer according to the mass ratio, and stir evenly; add an appropriate amount of sodium silicate, and continue stirring for 30 minutes until the slurry is uniform; S3, coating: evenly coating the prepared carbon coating slurry on the surface of the substrate; the coating thickness is controlled between 5-10 microns to ensure that the coating is uniform and dense; S4, drying and curing: placing the coated substrate into an oven for stage-by-stage drying and curing.

7. The method for using the highly conductive carbon-coated slurry for battery foil according to claim 6, characterized in that: The parameters of staged drying and curing in S4 are as follows: drying the coated substrate in stages at 60°C, 80°C and 100°C, with each stage drying time being 30 minutes; and finally drying at 120°C for 2 hours to ensure that the coating is completely cured.

Citation Information

Patent Citations

  • Water-based conductive paste and preparation method thereof

    CN113270233A

Cited By

  • Modified polyacrylic acid binder, carbon-coated aluminum foil and preparation methods of modified polyacrylic acid binder and carbon-coated aluminum foil

    CN121718286A