Method for smelting and casting large-size Cu-Ni-Si-Mg series copper alloy cast ingot in atmosphere
By adjusting the composition of the copper liquid and covering the particles with carbon protection in the atmospheric environment, the problem of uneven composition of Cu-Ni-Si-Mg copper alloy ingots was solved, and stable production and high-quality casting of large-sized ingots were achieved.
Patent Information
- Application Number
- CN202410988074.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-29
AI Technical Summary
When casting large-size Cu-Ni-Si-Mg copper alloy ingots in an atmospheric environment, the compositions of easily oxidized elements Si and Mg are uneven, resulting in different chemical compositions at the beginning and end of the ingot, affecting product quality. Existing technology It is difficult to meet the needs of industrial production.
The copper raw material is dissolved and heated under atmospheric atmosphere, covered with granular carbon for protection, the content of Ni and impurity elements is analyzed and adjusted, and metallic silicon and copper-magnesium master alloy are added to ensure the stability of Si and Mg. Through converter and holding furnace processing, the The liquid copper ingredients are mixed evenly and then cast.
It effectively ensures the stability of the chemical composition of large-size Cu-Ni-Si-Mg copper alloy ingots, improves product quality and industrialization process, and meets the stable production needs of large-size ingots in atmospheric environments.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper alloy casting, and in particular relates to a method for casting a large-size Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere. Background Art
[0002] With the continuous development of electronic technology in recent years, the application of Cu-Ni-Si-Mg copper alloys in microelectronics, automotive industry and medical industry has become more and more eye-catching. Cu-Ni-Si-Mg copper alloys have high yield strength, excellent stress fatigue resistance, good forming performance, and excellent performance that cannot be replaced by other metal materials. The stability of chemical composition directly affects the final performance of Cu-Ni-Si-Mg copper alloys. It is very important to control the stability of melting and casting of easily oxidized elements Si and Mg in atmospheric environment.
[0003] The casting process is a continuous and stable solidification crystallization process, especially when industrial production is used to cast large-size ingots of 200×620×8000mm. The casting duration is more than 120 minutes. During this process, the chemical composition of the copper liquid cannot change, otherwise the chemical composition of the head and the end of an ingot will be different, which will cause the performance of the final product to change, seriously affecting the product quality.
[0004] Studying atmospheric melting and casting technology of large-sized Cu-Ni-Si-Mg copper alloy ingots and realizing stable production of large-sized Cu-Ni-Si-Mg copper alloy ingots in atmospheric environment is an important way to improve the performance of Cu-Ni-Si-Mg copper alloys. At present, the industry uses vacuum melting, small-sized ingot production and other methods for industrial production, and its production cost and production efficiency cannot meet the needs of the existing market. It is very important to seek a stable and reliable atmospheric melting and casting process method for large-sized Cu-Ni-Si-Mg copper alloy ingots. Summary of the invention
[0005] In view of the problem of uneven alloy composition when casting large-sized Cu-Ni-Si-Mg copper alloy ingots with existing casting technology, the present invention provides a method for smelting and casting large-sized Cu-Ni-Si-Mg copper alloy ingots in an atmospheric atmosphere. The method can meet the requirements of melting and casting large-sized Cu-Ni-Si-Mg copper alloys in an atmospheric atmosphere, ensure the composition stability of easily oxidized elements Si and Mg, and improve the quality level and industrialization progress of Cu-Ni-Si-Mg copper alloys.
[0006] The present invention is achieved through the following technical solutions: A method for smelting and casting a large-size Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere, wherein the smelting and casting are performed in an atmospheric atmosphere, and specifically comprises the following steps: (1) After the copper raw material is dissolved into copper liquid, the temperature is continued to rise to 1260~1300℃, and a layer of granular carbon is covered on the surface; (2) Analyze the content of Ni and other impurity elements in the copper liquid and adjust the content of Ni and other impurity elements; (3) Transfer the copper liquid to the holding furnace, remove the slag after the converter, and analyze the content of main elements and other impurity elements; (4) According to the contents of the main elements and other impurity elements in step (3), metallic silicon is added to adjust the Si content. After the metallic silicon is completely dissolved, a copper-magnesium intermediate alloy is added to adjust the Mg content. After the metal addition is completed, the converter is mixed evenly; (5) After mixing evenly, turn off the power and let it stand, analyze the composition of the copper liquid, and add granular carbon; (6) Adjust the temperature of the molten copper and start casting to obtain a Cu-Ni-Si-Mg copper alloy ingot.
[0007] Furthermore, in step (1), the copper raw materials are Cu-Ni-Si-Mg copper alloy scraps and electrolytic copper. The Cu-Ni-Si-Mg copper alloy scraps are first added to the smelting furnace, and then the electrolytic copper is added after the Cu-Ni-Si-Mg copper alloy scraps are dissolved.
[0008] Furthermore, in step (1), the particle size of the granular carbon is 2-5 mm, the covering thickness is 100-150 mm, the moisture content of the granular carbon is less than 0.2%, and the burnout rate is less than 50% / 4h.
[0009] Furthermore, in step (4), the insulation temperature of the insulation furnace is 1280-1300°C.
[0010] Furthermore, in step (2), the Ni element is adjusted by using electrolytic nickel.
[0011] Furthermore, the converter speed of the holding furnace in step (3) is greater than 2000 kg / min.
[0012] Furthermore, the mass percentage of magnesium in the copper-magnesium master alloy in step (4) is 10-15%.
[0013] Furthermore, the casting temperature of step (6) is 1160-1180°C, the casting speed is 60-80 mm / min, the water flow rate is 30-50 m³ / h, and the vibration frequency is 60-80 times / min.
[0014] Furthermore, in step (6), the mass percentage composition of the Cu-Ni-Si-Mg copper alloy ingot is: Ni: 2-3%; Si: 0.4-0.8%; Mg: 0.05-0.3%, and the balance is Cu.
[0015] Furthermore, in step (6), the size of the Cu-Ni-Si-Mg copper alloy ingot is 200~250×600~680×8000~10000 mm.
[0016] Beneficial Effects The smelting and casting method of the present invention can meet the requirements of melting and casting of large-sized Cu-Ni-Si-Mg copper alloys in an atmospheric atmosphere, and the chemical composition content fluctuation at the head and tail ends of the ingot is small, which solves the problem of uneven composition of large-sized Cu-Ni-Si-Mg copper alloy ingots under atmospheric melting and casting, ensures the composition stability of easily oxidized elements Si and Mg, and improves the quality level and industrialization process of Cu-Ni-Si-Mg copper alloys. DETAILED DESCRIPTION
[0017] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.
[0018] Example 1 Raw materials: 3500kg Cu-Ni-Si-Mg copper alloy scraps, 130kg electrolytic nickel, 5200kg electrolytic copper, 45kg metallic silicon and 60kg copper-magnesium master alloy (magnesium content 15%); (1) First, add 3500kg of Cu-Ni-Si-Mg copper alloy scraps into the melting furnace. After it is completely dissolved, add electrolytic copper. After it is completely dissolved, heat it to 1280℃. The surface of the copper liquid is covered with φ2-5mm granular carbon with a thickness of 100mm for complete protection. (2) Analyze the content of Ni and other impurity elements in the copper liquid, add metallic nickel, and adjust the content of Ni and other impurity elements; (3) The copper liquid is transferred to a holding furnace (holding temperature 1280~1300℃), the converter speed is 2200kg / min, the converter time is 4min, and the copper liquid in the holding furnace is slag-stripped after the converter (power is turned off during slag-stripping). The surface of the copper liquid is covered with φ2-5mm granular carbon with a thickness of 100mm for complete protection; the content of main elements and other impurity elements is analyzed; (4) According to the content of the main element and other impurity elements in step (3), add metal silicon to adjust the Si content. After the metal silicon is completely dissolved, add copper-magnesium intermediate alloy to adjust the Mg content. After the metal addition is completed, the insulation furnace is sent to the converter for mixing for 5 minutes. (5) After the power supply is completed, the power is turned off and the copper liquid is allowed to stand. After 15 minutes, the composition of the copper liquid is analyzed and determined to be: Ni: 2.48%; Si: 0.49%; Mg: 0.15%; the remainder is Cu. Add φ2-5mm granular carbon to the holding furnace to maintain the granular carbon coverage thickness. ; (6) The temperature of the molten copper was adjusted and casting began. The casting temperature was 1170°C, the casting speed was 70 mm / min, the water flow rate was 35 m³ / h, and the vibration frequency was 60 times / min. A Cu-Ni-Si-Mg copper alloy ingot was cast with a cross-sectional size of 200×620 mm and a length of 8100 mm. Samples were taken at the head and end of the ingot for composition analysis. The contents of Si and Mg, which were easily oxidized elements, were 2.51% and 0.148% at the head end, and 2.50% and 0.147% at the end, respectively. No obvious changes were observed, and the composition control was stable.
[0019] Example 2 Raw materials: 3550kg Cu-Ni-Si-Mg copper alloy scraps, 128kg electrolytic nickel, 5150kg electrolytic copper, 50kg metallic silicon and 62kg copper-magnesium master alloy (magnesium content 15%); (1) First, add 3500kg of Cu-Ni-Si-Mg copper alloy scraps into the melting furnace. After it is completely dissolved, add electrolytic copper. After it is completely dissolved, heat it to 1278℃. The surface of the copper liquid is covered with φ2-5mm granular carbon with a thickness of 115mm for complete protection. (2) Analyze the content of Ni and other impurity elements in the copper liquid, add metallic nickel, and adjust the content of Ni and other impurity elements; (3) The copper liquid is transferred to a holding furnace (holding temperature 1280~1300℃), the converter speed is 2200kg / min, the converter time is 4min, and the copper liquid in the holding furnace is slag-stripped after the converter (power is turned off during slag-stripping). The surface of the copper liquid is covered with φ2-5mm granular carbon with a thickness of 150mm for complete protection; the content of main elements and other impurity elements is analyzed; (4) According to the content of the main element and other impurity elements in step (3), add metal silicon to adjust the Si content. After the metal silicon is completely dissolved, add copper-magnesium intermediate alloy to adjust the Mg content. After the metal addition is completed, the insulation furnace is sent to the converter for mixing for 5 minutes. (5) After the power supply is completed, the power is turned off and the copper liquid is allowed to stand. After 15 minutes, the composition of the copper liquid is analyzed and determined to be: Ni: 2.45%; Si: 0.52%; Mg: 0.145%; the remainder is Cu. Add φ2-5mm granular carbon to the insulation furnace to maintain the granular carbon coverage thickness. ; (6) The temperature of the molten copper was adjusted and casting began. The casting temperature was 1175°C, the casting speed was 80 mm / min, the water flow rate was 40 m³ / h, and the vibration frequency was 60 times / min. A Cu-Ni-Si-Mg copper alloy ingot was cast. The cross-sectional dimensions were 200×620 mm and the length was 8150 mm. Samples were taken at the head and end of the ingot for composition analysis. The contents of Si and Mg, which were easily oxidized elements, at the head end were 0.53% and 0.146%, respectively, and the contents of Si and Mg, which were easily oxidized elements at the end, were 0.51% and 0.145%, respectively. No obvious changes were observed, and the composition control was stable.
[0020] The above embodiments are only preferred examples of the present invention and are not intended to limit the present invention. Except for the technical features described in the specification, all other technical features are known to those skilled in the art.
Claims
1. A method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere, characterized in that: The smelting and casting is carried out in an atmospheric atmosphere, and specifically comprises the following steps: (1) After the copper raw material is dissolved into copper liquid, the temperature is continued to rise to 1260~1300℃, and a layer of granular carbon is covered on the surface; (2) Analyze the content of Ni and other impurity elements in the copper liquid and adjust the content of Ni and other impurity elements; (3) transferring the copper liquid to a holding furnace, removing the slag after the converter, and analyzing the content of the main element and other impurity elements; (4) adding metallic silicon to adjust the Si content according to the content of the main element and other impurity elements in step (3); after the metallic silicon is completely dissolved, adding a copper-magnesium intermediate alloy to adjust the Mg content; after the addition of the metal is completed, mixing the mixture evenly in the converter; (5) After mixing evenly, turn off the power and let it stand, analyze the composition of the copper liquid, and add granular carbon; (6) Adjust the temperature of the molten copper and start casting to obtain a Cu-Ni-Si-Mg copper alloy ingot.
2. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: In step (1), the copper raw materials are Cu-Ni-Si-Mg copper alloy scraps and electrolytic copper. The Cu-Ni-Si-Mg copper alloy scraps are first added to the smelting furnace, and then the electrolytic copper is added after the Cu-Ni-Si-Mg copper alloy scraps are dissolved.
3. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: In step (1), the particle size of the granular carbon is 2-5 mm, the covering thickness is 100-150 mm, the moisture content of the granular carbon is less than 0.2%, and the burning rate is less than 50% / 4h.
4. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: In step (4), the insulation temperature of the insulation furnace is 1280-1300°C.
5. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: In step (2), the Ni element is adjusted by using electrolytic nickel.
6. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: The converter speed of the holding furnace in step (3) is greater than 2000 kg / min.
7. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: The mass percentage of magnesium in the copper-magnesium master alloy of step (4) is 10-15%.
8. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: The casting temperature of step (6) is 1160-1180°C, the casting speed is 60-80 mm / min, the water flow rate is 30-50 m³ / h, and the vibration frequency is 60-80 times / min.
9. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: The mass percentage composition of the Cu-Ni-Si-Mg copper alloy ingot in step (6) is: Ni: 2-3%; Si: 0.4-0.8%; Mg: 0.05-0.3%, the balance is Cu.
10. The method for melting and casting a large-sized Cu-Ni-Si-Mg copper alloy ingot in an atmospheric atmosphere according to claim 1, characterized in that: The size of the Cu-Ni-Si-Mg copper alloy ingot in step (6) is 200~250×600~680×8000~10000mm.