Powder additive manufacturing method for nitrogen atom interstitial solution strengthening Ti2AlNb alloy
By using a mixed gas of nitrogen and argon for solid solution strengthening of nitrogen atom gaps during the additive manufacturing process, the problem of improving the mechanical properties of the Ti2AlNb alloy is solved, achieving efficient mechanical properties improvement and grain refinement of the alloy, and avoiding oxidation and Uneven stress problem.
Patent Information
- Application Number
- CN202410919985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology is difficult to effectively improve the mechanical properties of Ti2AlNb alloy during the additive manufacturing process, and there are problems such as element segregation, unfused metal powder and uneven stress distribution.
By passing a mixed gas of nitrogen and argon into the forming chamber, controlling the oxygen content below 100 ppm, preheating the substrate and using a laser beam to heat the Ti2AlNb-based alloy powder, nitrogen atoms enter the alloy lattice to achieve solid solution strengthening of the nitrogen atom gap. , regulating gas proportions and process parameters to improve mechanical properties.
It improves the mechanical properties of the alloy, prevents oxidation, reduces residual stress during the forming process, improves grain refinement and tensile strength, and avoids interlayer cracking and edge warping.
Smart Images

Figure CN118854104A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of titanium-aluminum alloy metal powder additive manufacturing, and more specifically, relates to a powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb alloy. Background Art
[0002] In recent years, with the rapid development of the aerospace field, the requirements for the mechanical properties and lightweight improvements of materials used in aerospace vehicles have become increasingly higher. The performance improvement and lightweight design of materials can not only increase the service life of the engine, but also reduce energy consumption.
[0003] Currently, the materials used in aerospace vehicles are mainly nickel-based alloys, but their high density limits their widespread use and promotion in engines. There is an urgent need to develop a high-strength lightweight material to replace nickel-based alloys.
[0004] As a lightweight material, titanium-aluminum alloy is expected to replace nickel-based alloys in the aerospace field. However, titanium-aluminum alloy is currently mainly manufactured by casting and forging, and is difficult to process due to its low plasticity. Therefore, additive manufacturing is a new technology that is expected to manufacture aircraft engine parts with complex structures.
[0005] Selective Laser Melting (SLM) technology is a rapidly developing new technology in Additive Manufacturing (AM) technology. It integrates multiple advanced manufacturing technologies, including computer-aided design, computer numerical control, material forming, etc. By setting the power of the high-energy laser beam, the scanning path and other process parameters, the metal powder in the set area is directly melted, and then accumulated layer by layer to form a three-dimensional solid part with a complex structure.
[0006] Ti2AlNb-based titanium aluminum alloy, as a new generation of titanium aluminum alloy, is considered to be a competitive material to replace nickel-based alloys due to its excellent mechanical properties. However, the improvement of mechanical properties has always been the pursuit of researchers. The current methods of alloy performance enhancement include element enhancement and particle enhancement. However, these two methods have the following defects: (1) The element enhancement process will lead to serious element segregation, which is not conducive to the uniformity of composition. (2) Due to the high melting point of the single element, there is unfused metal powder in the printing process, which is not conducive to the mechanical properties of the material. (3) The particle enhancement process will lead to uneven stress distribution, which is easy to cause interlayer cracking and edge warping. Summary of the invention
[0007] In view of the defects of the prior art, the object of the present invention is to provide a metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, so as to solve the technical problem of difficulty in improving the mechanical properties of Ti2AlNb alloy in the additive manufacturing process proposed in the above background technology.
[0008] To achieve the above object, the present invention provides a metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0009] (1) The forming chamber is evacuated, and then a mixture of nitrogen and argon is introduced to reduce the oxygen content in the chamber to less than 100 ppm; the formed substrate is then preheated;
[0010] (2) After the substrate reaches the preheating temperature, the dried Ti2AlNb-based alloy powder is evenly spread on the surface of the substrate;
[0011] (3) heating the alloy powder laid on the surface of the substrate to melt and shape it;
[0012] (4) Repeating steps (2) and (3) to obtain a pre-designed formed part, i.e., a Ti2AlNb-based alloy strengthened by interstitial solid solution of nitrogen atoms.
[0013] Preferably, in step (1), the volume ratio of the nitrogen in the mixed gas is less than or equal to 5%.
[0014] Preferably, the preheating temperature in step (2) is 150-200° C., and the temperature is kept constant at 150-200° C. during the printing process to reduce residual stress during the forming process.
[0015] Preferably, the composition of the Ti2AlNb-based alloy powder in step (2) is Ti 18-30 Al 12.5-30 Nb, powder particle size is 15-53μm.
[0016] Preferably, the dried Ti2AlNb-based alloy powder in step (2) is a Ti2AlNb-based alloy powder obtained by drying under vacuum conditions and / or an inert atmosphere.
[0017] Further preferably, in step (2), the Ti2AlNb-based alloy powder is dried in a vacuum drying oven at 80-120° C., and argon gas is introduced during the drying process to prevent oxidation of the powder, thereby obtaining a dried Ti2AlNb-based alloy powder.
[0018] Preferably, in step (2), the dried Ti2AlNb-based alloy powder is evenly spread on the surface of the substrate using a powder scraper or a powder feeder, and the powder spreading thickness is 20-40 μm. The excess powder on the surface is sent to the powder drop bin by the scraper.
[0019] Preferably, in step (3), a laser beam is used to heat the alloy powder laid on the surface of the substrate and melt and shape it.
[0020] Preferably, the laser beam used in step (3) has a laser power of 120-180 W and a scanning speed of 400-800 mm / s.
[0021] Preferably, the scanning path of the laser beam forming is from point to line by scanning line by line to melt the mixed powder, and the overlap distance between lines is set to 100-140 μm.
[0022] Preferably, during the melting and forming process of step (3), the oxygen content is controlled below 100 ppm to prevent the titanium aluminum alloy from being oxidized during the forming process.
[0023] According to another aspect of the present invention, there is provided a nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy prepared by the preparation method.
[0024] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0025] (1) The present invention provides a metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthening Ti2AlNb-based alloy. The method only changes the atmosphere in the forming chamber and introduces a certain proportion of N2. During the melting process, nitrogen atoms enter the lattice gap of the titanium aluminum alloy to produce a solid solution strengthening effect. It is not only simple to operate and low in cost, but also can achieve the effect of enhancing the mechanical properties of the alloy.
[0026] (2) The present invention achieves the effect of solid solution strengthening of Ti2AlNb-based alloys during additive manufacturing by regulating the ratio of nitrogen and argon in the mixed gas. At the same time, the addition of nitrogen increases the cooling rate of the molten metal, achieving the effect of grain refinement. The solid solution strengthening of nitrogen atoms causes the matrix lattice to be distorted, hinders the deformation of the grains during the stretching process, and greatly improves the mechanical properties of the alloy.
[0027] (3) The present invention evacuates the additive manufacturing forming chamber and then introduces a mixture of nitrogen and argon to keep the oxygen content in the chamber below 100 ppm, thereby preventing oxidation of the molten metal during the subsequent additive manufacturing process, which may cause cracking of the final formed part and affect the mechanical properties of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a microscopic mechanism diagram of the metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthening Ti2AlNb-based alloy in Example 1 of the present invention;
[0029] Figure 2This is a grain distribution diagram of a sample obtained by a metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthening Ti2AlNb-based alloy according to Example 1 of the present invention;
[0030] Figure 3 The mechanical properties diagram of the Ti2AlNb-based alloy samples prepared in Examples 1 to 3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0032] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0033] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0034] In the present invention, unless otherwise specified and / or described, all numerical values involving the amounts of components are "parts by weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions.
[0035] The present invention provides a powder additive manufacturing method for a Ti2AlNb alloy strengthened by interstitial solid solution of nitrogen atoms. The forming chamber is evacuated, and then a mixed gas of nitrogen and argon is introduced to make the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal; the forming substrate is preheated, and after the substrate reaches the preheating temperature, the dried Ti2AlNb-based alloy powder is evenly spread on the surface of the substrate; the alloy powder laid on the surface of the substrate is heated and melted to form; the powder spreading and forming steps are repeated to obtain a pre-designed alloy formed part, i.e., a Ti2AlNb-based alloy strengthened by interstitial solid solution of nitrogen atoms. The present invention dissolves nitrogen atoms in the titanium-aluminum alloy to achieve interstitial solid solution by adding an appropriate amount of N2, so that the titanium-aluminum alloy lattice is distorted, resulting in improved mechanical properties.
[0036] The following are examples:
[0037] Example 1
[0038] A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0039] (1) Drying the metal powder of Ti2AlNb-based alloy in a vacuum drying oven (temperature of 100°C) for half an hour, and introducing argon gas into the vacuum drying oven to prevent the powder from oxidizing; the metal powder composition of the Ti2AlNb-based alloy is: Ti 22 Al 25 Nb; powder particle size is 15-53μm.
[0040] (2) Use a vacuum pump to evacuate the forming chamber, and then introduce a mixture of nitrogen and argon (Ar:N2 volume ratio = 99:1) to keep the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal.
[0041] (3) First, the forming substrate is preheated using an external heat source (resistance wire). When the preheating temperature of the substrate reaches 170°C, powder is spread and formed. The temperature is kept constant at 170°C during the printing process.
[0042] (4) The powder is evenly spread on the surface of the substrate using a powder spreading scraper, and the powder is melted and formed under the heating of the laser beam. The powder spreading thickness is 30 μm. The laser power is 140 W, the scanning speed is 600 mm / s, and the scanning path of the laser beam forming is from point to line. The mixed powder is melted by scanning line by line, and the overlap distance between lines is set to 120 μm.
[0043] (5) Repeat step (4) to obtain a pre-designed formed part, i.e., a titanium-aluminum alloy strengthened by solid solution of nitrogen atoms.
[0044] Comparative Example 1
[0045] The other conditions were the same as those in Example 1, except that step (2) was conducted with 100% argon gas without nitrogen addition.
[0046] The nitrogen atom strengthening mechanism diagram of the titanium aluminum alloy prepared in Example 1 is as follows Figure 1 As shown, by introducing a certain proportion of N2 into the bin, nitrogen atoms enter the lattice gap of the titanium aluminum alloy during the melting process.
[0047] The titanium aluminum alloys prepared in Example 1 and Comparative Example 1 were characterized by EBSD ( Figure 2 ), it can be seen that the grain size of the titanium aluminum alloy prepared in this embodiment is reduced after the introduction of argon gas.
[0048] Example 2
[0049] A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0050] (1) Drying the metal powder of Ti2AlNb-based alloy in a vacuum drying oven (temperature of 100°C) for half an hour, and introducing argon gas into the vacuum drying oven to prevent the powder from oxidizing; the metal powder composition of the Ti2AlNb-based alloy is: Ti 22 Al 25 Nb; powder particle size is 15-53μm.
[0051] (2) Use a vacuum pump to evacuate the forming chamber, and then introduce a mixture of nitrogen and argon (Ar:N2 volume ratio = 97:3) to keep the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal.
[0052] (3) First, the forming substrate is preheated using an external heat source (resistance wire). When the preheating temperature of the substrate reaches 170°C, powder is spread and formed. The temperature is kept constant at 170°C during the printing process.
[0053] (4) The powder is evenly spread on the surface of the substrate using a powder spreading scraper, and the powder is melted and formed under the heating of the laser beam. The powder spreading thickness is 30 μm. The laser power is 140 W, the scanning speed is 600 mm / s, and the scanning path of the laser beam forming is from point to line. The mixed powder is melted by scanning line by line, and the overlap distance between lines is set to 120 μm.
[0054] (5) Repeat step (4) to obtain a pre-designed formed part, i.e., a titanium-aluminum alloy strengthened by solid solution of nitrogen atoms.
[0055] Example 3
[0056] A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0057] (1) Drying the metal powder of Ti2AlNb-based alloy in a vacuum drying oven (temperature of 100°C) for half an hour, and introducing argon gas into the vacuum drying oven to prevent the powder from oxidizing; the metal powder composition of the Ti2AlNb-based alloy is: Ti 22 Al 25 Nb; powder particle size is 15-53μm.
[0058] (2) Use a vacuum pump to evacuate the forming chamber, and then introduce a mixture of nitrogen and argon (Ar:N2 volume ratio = 95:5) to keep the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal.
[0059] (3) First, the forming substrate is preheated using an external heat source (resistance wire). When the preheating temperature of the substrate reaches 170°C, powder is spread and formed. The temperature is kept constant at 170°C during the printing process.
[0060] (4) The powder is evenly spread on the surface of the substrate using a powder spreading scraper, and the powder is melted and formed under the heating of the laser beam. The powder spreading thickness is 30 μm. The laser power is 140 W, the scanning speed is 600 mm / s, and the scanning path of the laser beam forming is from point to line. The mixed powder is melted by scanning line by line, and the overlap distance between lines is set to 120 μm.
[0061] (5) Repeat step (4) to obtain a pre-designed formed part, i.e., a titanium-aluminum alloy strengthened by solid solution of nitrogen atoms.
[0062] The tensile properties of the microstructures of the formed parts obtained under different nitrogen volume concentrations in Examples 1 to 3 and Comparative Example 1 are as follows: Figure 3 As shown, it can be seen that compared with Comparative Example 1, the tensile strength of the titanium aluminum alloy is effectively improved after adding nitrogen in Examples 1 to 3.
[0063] Example 4
[0064] A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0065] (1) Drying the metal powder of Ti2AlNb-based alloy in a vacuum drying oven (temperature of 120°C) for half an hour, and passing argon gas into the vacuum drying oven to prevent the powder from oxidation; the metal powder composition of the Ti2AlNb-based alloy is: Ti 22 Al 25 Nb; powder particle size is 15-53μm.
[0066] (2) Use a vacuum pump to evacuate the forming chamber, and then introduce a mixture of nitrogen and argon (Ar:N2 volume ratio = 95:3) to keep the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal.
[0067] (3) First, the forming substrate is preheated using an external heat source (resistance wire). When the preheating temperature of the substrate reaches 150°C, powder is spread and formed. The temperature is kept constant at 150°C during the printing process.
[0068] (4) The powder is evenly spread on the surface of the substrate using a powder spreading scraper, and the powder is melted and formed under the heating of the laser beam. The powder spreading thickness is 20 μm. The laser power is 120 W, the scanning speed is 400 mm / s, and the scanning path of the laser beam forming is from point to line. The mixed powder is melted by scanning line by line, and the overlap distance between lines is set to 100 μm.
[0069] (5) Repeat step (4) to obtain a pre-designed formed part, i.e., a titanium-aluminum alloy strengthened by solid solution of nitrogen atoms.
[0070] Example 5
[0071] A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, comprising the following steps:
[0072] (1) Drying the metal powder of Ti2AlNb-based alloy in a vacuum drying oven (temperature of 90° C.) for half an hour, and introducing argon gas into the vacuum drying oven to prevent oxidation of the powder; the metal powder composition of the Ti2AlNb-based alloy is: Ti 22 Al 25 Nb; powder particle size is 15-53μm.
[0073] (2) Use a vacuum pump to evacuate the forming chamber, and then introduce a mixture of nitrogen and argon (Ar:N2 volume ratio = 95:3) to keep the oxygen content in the chamber below 100 ppm to prevent oxidation and cracking of the molten metal.
[0074] (3) First, the forming substrate is preheated using an external heat source (resistance wire). When the preheating temperature of the substrate reaches 200°C, powder is spread and formed. The temperature is kept constant at 200°C during the printing process.
[0075] (4) The powder is evenly spread on the surface of the substrate using a powder spreading scraper, and the powder is melted and formed under the heating of the laser beam. The powder spreading thickness is 40 μm. The laser power is 180 W, the scanning speed is 800 mm / s, and the scanning path of the laser beam forming is from point to line. The mixed powder is melted by scanning line by line, and the overlap distance between lines is set to 140 μm.
[0076] (5) Repeat step (4) to obtain a pre-designed formed part, i.e., a titanium-aluminum alloy strengthened by solid solution of nitrogen atoms.
[0077] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A metal powder additive manufacturing method for nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy, characterized in that: The following steps are involved: (1) The forming chamber is evacuated, and then a mixture of nitrogen and argon is introduced to reduce the oxygen content in the chamber to less than 100 ppm; the formed substrate is then preheated; (2) After the substrate reaches the preheating temperature, the dried Ti2AlNb-based alloy powder is evenly spread on the surface of the substrate; (3) heating the alloy powder laid on the surface of the substrate to melt and shape it; (4) Repeating steps (2) and (3) to obtain a pre-designed formed part, i.e., a Ti2AlNb-based alloy strengthened by interstitial solid solution of nitrogen atoms.
2. The preparation method according to claim 1, characterized in that In step (1), the volume ratio of the nitrogen in the mixed gas is less than or equal to 5%.
3. The preparation method according to claim 1, characterized in that: The preheating temperature in step (2) is 150-200°C.
4. The preparation method according to claim 1, characterized in that: The composition of the Ti2AlNb-based alloy powder in step (2) is Ti 18-30 Al 12.5-30 Nb, powder particle size is 15-53μm.
5. The preparation method according to claim 1, characterized in that: Step (2) The dried Ti2AlNb-based alloy powder is evenly spread on the surface of the substrate, and the powder thickness is 20-40 μm.
6. The preparation method according to claim 1, characterized in that: In step (3), a laser beam is used to heat the alloy powder laid on the surface of the substrate and melt it into shape.
7. The preparation method according to claim 6, characterized in that: The laser beam used in step (3) has a laser power of 120-180 W and a scanning speed of 400-800 mm / s.
8. The nitrogen atom interstitial solid solution strengthened Ti2AlNb-based alloy prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
High-temperature alloy additive manufacturing method
CN107790720A
Cited By
Method for additive forming of high-performance Ti2AlNb three-period minimal curved surface lattice structure in nitrogen atmosphere
CN120542073A
Titanium-aluminum-based alloy destressing additive manufacturing method
CN120587490A