Ultrahigh-strength steel plate with excellent cold bending performance and manufacturing method thereof
Through specific chemical composition and process flow, the problem of insufficient cold-bending performance of ultra-high-strength steel plates in the existing technology has been solved, and the production of ultra-high-strength steel plates with a yield strength greater than 1500MPa, a tensile strength of nearly 1800MPa and excellent cold-bending properties has been achieved, which is suitable for in engineering machinery and other fields.
Patent Information
- Application Number
- CN202411062290.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to mass-produce ultra-high-strength steel plates with a yield strength of more than 1,500MPa, a tensile strength of nearly 1,800MPa, and excellent cold-bending properties using existing technology, and the process is not suitable for common domestic flat rolling equipment.
Use specific chemical composition, such as C: 0.25~0.35, Si: 0.10~0.40, Mn: 0.50~1.50, Cr: 0.30~1.00, Mo: 0.20~0.60, Ni: 1.00~2.00, Nb: 0.01~0.03, V: 0.01~0.03, Al: 0.04~0 .08, P≤0.010, S≤0.003, O: ≤0.0008, N: 0.0020-0.0045, H: ≤0.0001 steel plate, by rotating Furnace smelting, LF refining, RH vacuum degassing, low superheat argon protected casting, double-stand rolling and quenching + low temperature tempering heat treatment processes ensure the high strength and excellent cold bending performance of the steel plate.
The yield strength of the 4-30mm steel plate is greater than 1500MPa, the tensile strength is greater than 1650MPa, the elongation is ≥8%, and the Charpy impact energy at -40℃ is ≥20J. The excellent performance of the cold bending radius avoids the cold bending process of the steel plate. cracking problem.
Smart Images

Figure CN118854162A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of special steel smelting, and in particular relates to an ultra-high-strength steel plate with excellent cold bending performance and a manufacturing method thereof. Background Art
[0002] As a modern lightweight steel material, high-strength steel plates are widely used in the fields of engineering machinery, special vehicles and equipment, such as the booms of large equipment and the beams of large-tonnage vehicles. At present, the domestic standard for high-strength steel plates generally uses GB / T 16270-2009, which stipulates that the yield strength of the highest strength quenched and tempered steel plates is 960MPa. With the improvement of equipment manufacturing and welding levels, domestic special steel companies represented by Xingcheng Special Steel have developed steel plates with a yield strength of 1100MPa and applied them in batches to domestic special equipment manufacturing companies. Ultra-high-strength steel plates with a yield strength higher than 1100MPa are generally in the research and development stage and have not been used in batches. Among them, research and development is mainly focused on the yield strength of 1100-1300MPa.
[0003] Chinese patent CN113430467A introduces a thin gauge 1400MPa grade bainitic steel and its manufacturing method. The steel coil produced has a tensile strength of ≥1400MPa, an elongation after fracture of ≥13%, and a thickness of 0.8-1.8mm. This thickness is limited in application on large-scale engineering machinery and equipment. Chinese patent CN104532156A reports a 1300MPa grade modulated high-strength steel with a yield strength of no more than 1400MPa and a tensile strength of more than 1500MPa. The strength level is low, and the product is delivered in coils. The process is not suitable for the more common flat rolling equipment in China, and the processing performance of the material is not further described. This patent aims to provide an ultra-high strength steel plate with a yield strength of more than 1500MPa, a tensile strength of nearly 1800MPa, and excellent cold bending performance. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a 4-30mm ultra-high strength steel plate with excellent cold bending performance, a yield strength greater than 1500MPa and a manufacturing method thereof in accordance with the above-mentioned prior art. The main mechanical properties of the steel plate are: yield strength > 1500MPa, tensile strength > 1650MPa, elongation ≥ 8%; -40℃ Charpy impact energy ≥ 20J; 90° cold bending radius of the steel plate: for steel plates with thickness ≤ 8mm, the cold bending radius ≥ 3t; for steel plates with thickness 8<≤15mm, the cold bending radius ≥ 4t; for steel plates with thickness 15<≤30mm, the cold bending radius ≥ 6t.
[0005] The technical solution adopted by the present invention to solve the above problems is: an ultra-high strength steel plate with excellent cold bending performance, the chemical composition of the steel and its mass percentage are: C: 0.25-0.35, Si: 0.10-0.40, Mn: 0.50-1.50, Cr: 0.30-1.00, Mo: 0.20-0.60, Ni: 1.00-2.00, Nb: 0.01-0.03, V: 0.01-0.03, Al: 0.04-0.08, P≤0.010, S≤0.003, O:≤0.0008, N: 0.0020-0.0045, H:≤0.0001, and the rest are Fe and unavoidable impurities.
[0006] The following is a detailed description of the effects and dosage of the components in the present invention:
[0007] C: The carbon content has a great influence on the strength level and low temperature toughness of the steel plate. The higher the carbon content, the more complete the quenching martensite transformation, the higher the strength of the steel plate, but the toughness and plasticity will be reduced; the lower the carbon content, the better the toughness of the steel plate, but the hardenability of the steel plate is reduced, which is not conducive to the strengthening of the martensite phase to obtain ultra-high strength. Based on the strength and toughness matching of the steel plate, the present invention controls the carbon content to 0.25-0.35%.
[0008] Si: Silicon is an important deoxidizing element in steel. An appropriate amount of silicon can improve the elastic limit, yield point and tensile strength of steel. Too high a content will deteriorate the toughness of martensitic high-strength steel, which is detrimental to the cold bending performance of the material and reduces the surface quality of the steel plate. The silicon content of the present invention is controlled to be 0.10-0.40%.
[0009] Mn: Manganese is a commonly used solid solution strengthening element. It has the effect of delaying the transformation of austenite to ferrite in steel and promoting martensite transformation. However, if the manganese content is too high, it is easy to cause segregation, reduce the toughness of the material, and deteriorate the performance of the steel plate. The manganese content of the present invention is controlled to be 0.50-1.50%.
[0010] Cr: Chromium is an element that improves the hardenability of steel, can inhibit the formation of polygonal ferrite and pearlite, promote the transformation of low-temperature microstructures bainite or martensite, and improve the strength of the steel plate. The chromium content of the present invention is controlled at 0.30-1.00%.
[0011] Mo: Molybdenum can improve the hardenability of the material. Adding a certain amount of molybdenum will increase the strength of the steel plate without affecting the low-temperature impact performance of the steel plate. In the present invention, the content of molybdenum is controlled at 0.20-0.60%.
[0012] Ni: Nickel can increase the hardenability of steel. The addition of nickel is beneficial to improving the cold working performance of the material and the performance of the welding joint. The content of nickel in the present invention is controlled to be 1.00-2.00%.
[0013] Al: Aluminum is a strong deoxidizing element and an important element for refining grains. The aluminum content is controlled within the range of 0.04-0.08% in the present invention.
[0014] Nb and V: Niobium and vanadium are both microalloying elements, which form nano-scale precipitates with carbon, nitrogen and other elements in steel. Niobium can increase the non-recrystallization temperature and expand the rolling window; vanadium can effectively improve the strength of the material in tempered steel. The present invention stipulates that the niobium content is 0.01-0.03%; the vanadium content range is 0.01-0.03%.
[0015] P: Phosphorus is an impurity element in steel, which is easy to form intergranular segregation, which has an adverse effect on the toughness of high-strength steel plates, and its content should be reduced as much as possible. In the present invention, phosphorus is controlled to be no more than 0.010%.
[0016] S: Sulfur is generally a harmful element in steel. It is easy to exist in the steel as sulfide inclusions, reducing the ductility and toughness of the steel. In the present invention, the sulfur content is controlled to be no more than 0.003%.
[0017] H, O: Hydrogen and oxygen are both harmful gas elements. Hydrogen easily causes white spots in steel. Too high a content of hydrogen can cause ultra-high strength steel plates to crack easily. The higher the oxygen content, the more inclusions there are, which reduces the plasticity, toughness and bending properties of the steel plate. The present invention strictly controls the hydrogen content to be no more than 0.0001% and the oxygen content to be no more than 0.0008%.
[0018] N: Nitrogen is generally a harmful gas element. A proper amount of nitrogen helps microalloy elements such as aluminum and niobium to form microalloys that hinder grain growth, and helps to improve the strength, toughness and cold bending performance of the material. Combined with the microalloy design content of the present invention, the nitrogen content of the present invention is 0.0020-0.0045%.
[0019] The manufacturing method of the above-mentioned 4-30 mm ultra-high strength steel plate mainly comprises the following steps:
[0020] 1. Steelmaking
[0021] The molten steel is smelted in a converter and then refined in an LF refining furnace. After refining, the first stage of Ca treatment is carried out, and high vacuum treatment is carried out in an RH vacuum degassing furnace. The vacuum degree is required to be no higher than 67Pa and the treatment time is no less than 35min to ensure that the H content in the molten steel is within the target requirement. Properly increasing the molten steel degassing time is also conducive to the contact rate between Ca and inclusions and improving the purity of the molten steel. After breaking the air, the second stage of Ca treatment is carried out, and the remaining Ca wire is fed. During this period, samples are taken for N content analysis. When the content is less than the lower limit of the target, nitrogen blowing is required to increase nitrogen. After Ca treatment, the molten steel is subjected to bottom argon soft stirring, and the stirring time is not less than 12 minutes to ensure that the inclusions are fully denatured and float.
[0022] 2. Continuous Casting
[0023] The casting adopts low superheat and argon protection casting, requiring the superheat of molten steel to be 10-20℃. Electromagnetic stirring and dynamic light pressure reduction technology are used at the end of molten steel solidification. The minimum pressure reduction of the mushy zone at the end of solidification is 3mm, and finally cast into 150mm thick continuous casting slab. Low-magnification samples are taken from the continuous casting slabs of each furnace of steel online to inspect the center segregation of the slabs. The slabs cut and segmented online are stacked into pits or covered for slow cooling. The target slow cooling temperature of the slab is 650±50℃, and the target slow cooling time in this temperature range is ≥12 hours, aiming to achieve the purpose of hydrogen expansion and help improve the processing performance of the final finished steel plate.
[0024] 3. Rolling
[0025] Continuous casting slabs with a center segregation of no more than Class C 1.0 are selected for heating and rolling, and heated to 1200-1250°C. The slabs are heated to temperature and kept warm for no less than 2 hours to ensure full solid solution of alloy elements and slow down segregation. A double-stand two-stage controlled rolling process is adopted. After the steel billet is removed from the furnace, it is descaled with high-pressure water and then subjected to "rough rolling + finishing rolling" to achieve two-stage controlled rolling. The starting rolling temperature of the rough rolling is ≥1000℃, and the reduction rate of the last two passes of the rough rolling is required to be ≥13%. The waiting thickness is ≥2.0H, where H is the finished product thickness. The purpose of high-temperature and large deformation rolling of the rough rolling is to improve the quality of the core of the steel plate and refine the grains; the starting target temperature of the finishing rolling is 860-940℃, and the steel plate is rolled into a steel plate after 3-8 passes. The rolled steel plate is cooled on a cooling bed after a hot straightening machine. When the steel plate is cooled to 300±50℃, it returns to the hot straightening machine for straightening treatment to avoid large curvature of the hot-rolled steel plate and ensure that the hot-rolled steel plate can be subsequently heated in a continuous furnace and quenched.
[0026] 4. Heat treatment
[0027] The steel plate undergoes quenching + low-temperature tempering heat treatment, the quenching temperature is 880±20℃, and the steel plate is heated to temperature and kept warm for 30-80min; after heating, it is quickly water-cooled to room temperature in a quenching machine to ensure uniform quenched martensite structure; the quenched steel plate needs to be low-temperature tempered, the tempering temperature is 180±20℃, the holding time is 40-200min, and after heating, it is air-cooled to room temperature on a cooling bed. This tempering process helps to release stress without reducing strength, which helps to improve the cold bending performance of the material; after low-temperature tempering, the steel plate is subjected to strong straightening treatment, the purpose is to further release the stress of the steel plate and ensure that the unevenness of the steel plate is ≤3mm / m.
[0028] Compared with the prior art, the advantages of the present invention are:
[0029] The composition of the ultra-high strength steel plate of 4-30 mm with excellent cold bending performance and yield strength greater than 1500 MPa is designed as C: 0.25-0.35, Si: 0.10-0.40, Mn: 0.50-1.50, Cr: 0.30-1.00, Mo: 0.20-0.60, Ni: 1.00-2.00, Nb: 0.01-0.03, V: 0.01-0.03, Al: 0.04-0.08, P≤0.010, S≤0.003, O:≤0.0008, N: 0.0020-0.0045, H:≤0.0001, and the rest is Fe and unavoidable impurities. In the composition design, a higher content of the commonly used element Al is used for microalloying, and a small amount of Nb and V are used for composite strengthening of the microalloy. The composition design requires N content within a certain range, aiming to fully and effectively exert the precipitation strengthening effect of the microalloy, achieve grain refinement, and improve the strength and toughness of the steel plate.
[0030] The composition design of the present invention strictly requires the content of O and H, in order to ensure the cold bending performance of the final steel plate and avoid cracking at a smaller cold bending angle. During the steelmaking process, two Ca treatments, high vacuum long-term treatment, and soft argon blowing long-term stirring treatment are used to achieve sufficient removal of inclusions in molten steel and limit the content of harmful gases O and H.
[0031] The present invention strictly controls the superheat of molten steel during molten steel casting, requiring the superheat of molten steel to be 10-20°C, in order to improve the low-multiple quality of the continuous casting slab, and requires electromagnetic stirring and dynamic light reduction technology to be used at the end of the molten steel solidification. The minimum reduction in the mushy zone at the end of the solidification is 3mm, which helps to slow down the segregation and loosening of the continuous casting slab.
[0032] The present invention requires that the continuous casting slabs be stacked into a pit or covered for slow cooling after coming off the line, and the target slow cooling temperature of the slabs is 650±50°C, and the target slow cooling time in this temperature range is ≥12 hours, in order to achieve the purpose of hydrogen expansion and help improve the processing performance of the final finished steel plate.
[0033] The present invention selects high-quality billets for steel plate rolling, requires that the center segregation of the ingot is not higher than Class C 1.0, and requires that the ingot be heated to a temperature and the holding time is not less than 2 hours, in order to ensure that the alloy elements are fully dissolved and segregation is slowed down.
[0034] The present invention adopts a double-frame two-stage controlled rolling process. The rolled steel plate is cooled on a cooling bed after passing through a hot straightening machine. When the steel plate is cooled to 300±50°C, it returns to the hot straightening machine for straightening treatment, thereby avoiding large buckling of the hot-rolled steel plate and ensuring that the hot-rolled steel plate can be subsequently heated in a continuous furnace and quenched.
[0035] The steel plate of the present invention is subjected to quenching + low temperature tempering heat treatment, and is required to be subjected to strong straightening treatment after tempering to further release the stress of the steel plate and achieve a steel plate unevenness of ≤3mm / m. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a 200-fold metallographic structure diagram of the core of a 25 mm thick steel plate in an embodiment of the present invention.
[0037] Figure 2 This is a test result diagram of cold bending 90° and 180° of a 4 mm thick steel plate in an embodiment of the present invention. The radius of the bending center is
[0038] 10mm. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0040] The main production process of the 4-30 mm ultra-high strength steel plate with excellent cold bending performance and yield strength greater than 1500 MPa is: converter steelmaking → LF refining → RH degassing → continuous casting → billet slow cooling → heating → rolling → quenching + tempering.
[0041] Examples 1-2 correspond to the production of steel plates with a thickness of 4 mm and 25 mm, respectively, and the main steps are as follows:
[0042] Smelting: The molten steel is smelted in a converter, and after LF refining, RH vacuum degassing is carried out. During the smelting process, Ca treatment is carried out in stages, and calcium wire is fed after LF refining and RH degassing respectively. After the second feeding of calcium wire treatment, bottom blowing argon soft stirring is carried out, and the stirring time is not less than 12 minutes. Considering the nitrogen addition of molten steel during casting, the N content of molten steel is controlled at 0.0020-0.0035% before casting. The composition of molten steel after smelting is shown in Table 1.
[0043] Continuous casting: Molten steel is continuously cast into 150mm thick continuous casting slabs by a straight arc continuous casting machine. The superheat of the cast steel is 10-20℃. Dynamic soft reduction and tundish heating technology are used in the continuous casting process. The minimum reduction in the mushy zone at the end of solidification is 3mm. After continuous casting, the slabs are tested by taking low-magnification samples. Only the slabs that meet the "center segregation C class not greater than 1.0 level" can be produced later. The continuous casting process parameters are shown in Table 2.
[0044] Slow cooling of billets: The slabs cut and segmented online are stacked and put into a pit or covered for slow cooling. The target slow cooling temperature of the slabs is 650±50℃. The target slow cooling time in this temperature range is ≥12 hours. The slow cooling process parameters are shown in Table 3.
[0045] Rolling: The continuous casting billet is heated to 1200-1250℃ by a continuous heating furnace, and the holding time of the slab after heating to temperature is not less than 2 hours. After the billet is removed from the furnace, it is descaled by high-pressure water and then subjected to "rough rolling + finishing rolling" to achieve two-stage controlled rolling. The starting rolling temperature of the rough rolling is ≥1000℃, and the reduction rate of the last two passes of the rough rolling is required to be ≥13%, and the waiting thickness is ≥2.0H, where H is the finished product thickness; the starting rolling target temperature of the finishing rolling is 860-940℃, and it is rolled into a steel plate after 3-8 passes. The rolled steel plate is cooled on the cooling bed after the hot straightening machine. When the steel plate cools to 300±50℃, it returns to the hot straightening machine for straightening treatment. The relevant process parameters are shown in Table 4.
[0046] Heat treatment + straightening: The steel plate is heat treated with "quenching + low temperature tempering", the quenching temperature is 880±20℃, the steel plate is heated to temperature and kept warm for 30-80min; after heating, it is quickly water-cooled to room temperature in a quenching machine; the quenched steel plate is subjected to low temperature tempering treatment, the tempering temperature is 180±20℃, the holding time is 40-200min, and after heating, it is air-cooled to room temperature on a cooling bed; after low temperature tempering, the steel plate is subjected to strong straightening treatment to achieve a steel plate unevenness of ≤3mm / m. The heat treatment process parameters are shown in Table 5.
[0047] The specific chemical composition and process parameters of Examples 1-2 are shown in Tables 1-4, and the mechanical and cold bending properties of the steel plates are shown in Table 6.
[0048] Table 1 Chemical composition of the examples (wt%)
[0049]
[0050] Table 2 Continuous casting process parameters
[0051] Example Thickness of ingot (mm) Superheat℃ Soft pressure at the end of solidification (mm) 1 150 16 3.3 2 150 14 3.5
[0052] Table 3 Billet slow cooling process parameters
[0053] Example Slow cooling start temperature ℃ Target temperature slow cooling time h 1 680 16 2 690 17
[0054] Table 4 Steel rolling process parameters
[0055]
[0056] Table 5 Heat treatment process parameters
[0057] Example Quenching temperature℃ Insulation time min Tempering temperature℃ Insulation time min 1 882 30 180 40 2 890 50 190 180
[0058] Table 6 Mechanical and cold bending properties
[0059]
[0060] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An ultra-high strength steel plate with excellent cold bending performance, characterized in that: The chemical composition of the steel plate and its mass percentage are C: 0.25-0.35, Si: 0.10-0.40, Mn: 0.50-1.50, Cr: 0.30-1.00, Mo: 0.20-0.60, Ni: 1.00-2.00, Nb: 0.01-0.03, V: 0.01-0.03, Al: 0.04-0.08, P≤0.010, S≤0.003, O:≤0.0008, N: 0.0020-0.0045, H:≤0.0001, and the rest are Fe and unavoidable impurities.
2. The ultra-high strength steel plate with excellent cold bending performance according to claim 1, characterized in that: The steel plate has a thickness of 4-30 mm, a yield strength of more than 1500 MPa, a tensile strength of more than 1650 MPa, an elongation of ≥8%, and a Charpy impact energy of ≥20 J at -40°C.
3. The ultra-high strength steel plate with excellent cold bending performance according to claim 2, characterized in that: The cold bending radius of the steel plate bending at 90°: for steel plates with thickness ≤8mm, the cold bending radius shall be ≥3t; for steel plates with thickness 8<≤15mm, the cold bending radius shall be ≥4t; for steel plates with thickness 15<≤30mm, the cold bending radius shall be ≥6t, where t represents the thickness of the steel plate.
4. A method for manufacturing an ultra-high strength steel plate with excellent cold bending performance as claimed in claim 1, characterized in that: The method comprises the following steps: (1) Smelting: The molten steel is smelted in a converter, and then subjected to RH vacuum degassing after LF refining; (2) Continuous casting: The molten steel is continuously cast into a 150 mm thick continuous casting slab by a straight arc continuous casting machine; (3) Slow cooling of billets: The slabs cut and segmented online are stacked and put into a pit or covered for slow cooling; (4) Rolling: The continuous casting slab is heated to 1200-1250°C in a continuous heating furnace. The slab is kept warm for no less than 2 hours after being heated to room temperature. After the slab is removed from the furnace, it is descaled by high-pressure water and then rolled in two stages. (5) Heat treatment + straightening: The steel plate undergoes "quenching + low temperature tempering" heat treatment. After low temperature tempering, the steel plate is subjected to strong straightening treatment to achieve a steel plate unevenness of ≤3mm / m.
5. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (1), Ca treatment is carried out in stages during the molten steel smelting process, and calcium wire is fed after LF refining and RH degassing respectively. After the second calcium wire feeding treatment, bottom argon soft stirring is carried out, and the stirring time is not less than 12 minutes. The N content of the molten steel is controlled at 0.0020-0.0035% before casting.
6. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (2), the superheat of the cast steel liquid is 10-20°C. During the continuous casting process, dynamic soft reduction and tundish heating technology are used, and the minimum reduction in the mushy zone at the end of solidification is 3 mm.
7. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (3), the segmented slabs are stacked and put into a pit or covered for slow cooling, and hydrogen expansion treatment is performed. The target slow cooling temperature of the slabs is 650±50°C, and the target slow cooling time in this temperature range is ≥12 hours.
8. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (4), the starting rolling temperature of rough rolling is ≥1000°C, the reduction ratio of the last two passes of rough rolling is ≥13%, and the waiting thickness is ≥2.0H, where H is the finished product thickness; the starting target temperature of finishing rolling is 860-940°C, and the steel plate is rolled into a steel plate through 3-8 passes.
9. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (5), the rolled steel plate passes through the hot straightening machine and then is cooled on a cooling bed. When the steel plate is cooled to 300±50° C., it is returned to the hot straightening machine for straightening treatment.
10. The method for manufacturing an ultra-high strength steel plate with excellent cold bending performance according to claim 4, characterized in that: In step (5), the quenching temperature of the steel plate is 880±20°C, and the steel plate is heated to temperature and kept warm for 30-80 minutes; after heating, it is quickly water-cooled to room temperature in a quenching machine; the quenched steel plate is subjected to low-temperature tempering treatment, the tempering temperature is 180±20°C, the insulation time is 40-200 minutes, and after heating, it is air-cooled to room temperature on a cooling bed.