Preparation method of antimicrobial nanofiber polymer material

By loading singlet oxygen and antibacterial active molecules in the bio-based nanofiber membrane, and using electrospinning technology to prepare antimicrobial nanofiber polymer materials, the problems of long exposure time of antibacterial materials and drug-resistant bacteria in the existing technology are solved, and the problem is achieved Fast and effective microbial killing and good mechanical properties.

CN118854485APending Publication Date: 2024-10-29JIANGSU SUPERVISION & INSPECTION INST FOR PROD QUALITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895591.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing photoactive polymer materials require a long exposure time to stimulate antibacterial activity, which limits their use in practical applications and makes it difficult to effectively remove drug-resistant strains.

Method used

Electrospinning technology is used to load singlet oxygen (O2(⁠Ag) and antibacterial active molecule ε-polylysine in bio-based nanofiber membranes, and antimicrobial nanofiber polymers are prepared through high-temperature melt polymerization and alternating assembly technology. Materials, combined with electrospinning technology, achieve nano- and sub-micron size layered structure design.

Benefits of technology

It achieves rapid and effective microbial killing ability, maintains the activity of bioactive molecules and the three-dimensional structure of the nanofiber template, has ultra-high specific surface area and good air permeability, and is suitable for packaging materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of an antimicrobial nanofiber polymer material, which comprises the following steps: taking citric acid and 1, 8-octylene glycol in a molar ratio of 1: 1, carrying out high-temperature melt polymerization reaction, cooling to 135-142 DEG C after the reaction monomers citric acid and 1, 8-octylene glycol are completely melted in an oil bath at 150-160 DEG C, reacting for 1-1.5 hours under a vacuum condition, filtering, washing, and drying to obtain the antimicrobial nanofiber polymer material. Dialyzing a reaction product with deionized water for 48 hours, and freeze-drying; the preparation method comprises the following steps: completely dissolving 0.5 mmol of poly citrate (PC) in 10mL of dimethyl sulfoxide; adding 2.5 mmol of EDC (Ethylene Dichloride), and uniformly stirring; 1 mmol of NHS is added, and stirring is carried out; adding antibacterial active molecules, and stirring; dialyzing the product in deionized water, and freeze-drying to obtain a PCE polymer; after EDC is added, stirring is conducted for 30 min at the temperature of 25 DEG C; nHS is added, and stirring is conducted for 12 h at the temperature of 25 DEG C; adding antibacterial active molecules, and stirring at the temperature of 25 DEG C; according to the invention, active molecules are loaded in a bio-based nanofiber membrane by adopting an electrostatic spinning technology, and a novel packaging material capable of preventing and controlling generation of hazardous substances is developed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanofiber polymers, and in particular to a method for preparing an antimicrobial nanofiber polymer material. Background Art

[0002] With the increasing incidence of viral and bacterial infections, often caused by resistant strains and more10 often also associated with the so-called nosocomial infection problem, a global health problem, the search for new microbicidal methods is becoming increasingly important. Therefore, the use of special photoactive dyes (so-called photosensitizers) that generate singlet oxygen (O2(Ag)) in a photosensitized reaction has attracted great interest, mainly due to the high reactivity of O2(Ag) and the associated cytotoxicity. This cytotoxicity is used for the so-called photodynamic inactivation (PDI) of bacteria, viruses, yeast15 and protozoa. A significant advantage of PDI is that pathogens do not develop resistance to singlet oxygen. The photosensitized production of singlet oxygen O2(Ag) usually takes place in a liquid phase, in which the photosensitizer is dissolved. However, this does not allow the photosensitizer to be easily separated from the treated object or product after the photoreaction. When the photosensitizer is anchored to a solid20 carrier, it can be easily separated from the reaction product and reused. In addition, as the surface area of ​​the carrier increases, the desired effect can be achieved with a smaller amount or a lower concentration of the photosensitizer in the carrier. By encapsulating a hydrophobic photosensitizer in polymer nanofibers, the specific properties of the photogenerator 02(Ag) (oxidation, cytotoxic effect, "in situ" activity) are combined with the specific properties of nanofibrous membranes from suitable polymers 25 (light transmission, easy oxygen diffusion, large specific surface area). The nanoporous structure of the nanofibrous membrane allows the effective capture of bacteria, viruses and other pathogens. The diffusion path of 02(Ag) is at most hundreds of nanometers. In previous studies, it has been found that nanofibrous polymer membranes with encapsulated photosensitizers can be prepared by the "electrospinning" method. The thickness 30 of these membranes is about 0.03 mm, the area weight is about 2 g / m2, the average diameter of the nanofibers is in the range of 100-400 nm, the photosensitizer is encapsulated, and it is characterized by UV-VIS, fluorescence and time-resolved spectroscopy.

[0003] For effective use in a variety of practical applications, suitable parameters still need to be determined and provided to provide cost-effective useful materials with minimal or no undesirable influencing factors. For applications where disinfection of a wider range of membrane environments is required, the photogeneration of singlet oxygen can be combined with the (photo)generation of other antimicrobial substances. However, such combinations only increase the number of problems with the practical use of these technologies. Existing photoactive polymer materials) are suboptimal and, in particular, they require15 relatively long exposure times to stimulate sufficient antimicrobial activity, which may prevent or significantly limit the use of these materials in practice. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing an antimicrobial nanofiber polymer material, using electrostatic spinning technology to load active molecules in a bio-based nanofiber membrane to develop a new type of packaging material that can prevent and control the generation of harmful substances.

[0005] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing an antimicrobial nanofiber polymer material, comprising the following steps:

[0006] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, the reaction monomers citric acid and 1,8-octanediol are completely melted in an oil bath at 150-160° C., then cooled to 135-142° C., reacted under vacuum conditions for 1-1.5 hours, the reaction product was dialyzed with deionized water for 48 hours, and freeze-dried;

[0007] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0008] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0009] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0010] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 155-160° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 135-140° C., and reacted under vacuum conditions for 1-2 hours.

[0011] Specifically, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is (0.1-10):1.

[0012] Specifically, after step S4, the following steps are also included:

[0013] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0014] Specifically, in step S5, the mass ratio of PCE polymer to the mixture is (0.1-0.6):1.

[0015] Furthermore, in step S5, the spinning solution solvent used in electrospinning is a mixture of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixture is (0.8-0.9):1.

[0016] Furthermore, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0017] Specifically, the parameters of the electrospinning are as follows: positive high voltage 5kv~19kv, negative high voltage 1kv~5kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 8cm~22cm, the spinning liquid propulsion speed is 0.1~0.19mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 35%~75%.

[0018] Specifically, after step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

[0019] Specifically, in step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling;

[0020] After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.

[0021] The method for preparing an antimicrobial nanofiber polymer material provided by the present invention has the following advantages compared with the prior art:

[0022] (1) The antimicrobial nanofiber polymer material obtained by the above preparation method; the preparation method of the present invention is simple, easy to operate, and has low raw material cost;

[0023] (2) Through simple alternating assembly technology, nano- and submicron-sized layered structures are designed on the surface of nanomaterials. The electrostatic self-assembly modified nanofiber structure is stable and does not destroy the activity of bioactive molecules. In addition, this method can effectively maintain the three-dimensional microstructure of the nanofiber template material. The structure has an ultra-high specific surface area and good air permeability, which greatly improves the activity of bioactive molecules and can be widely used in packaging materials. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments.

[0025] Example 1

[0026] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0027] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in a 150° C. oil bath, the temperature is lowered to 135° C., and the reaction is carried out under vacuum conditions for 1 hour, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0028] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0029] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0030] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0031] In this embodiment, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 155° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 135° C., and reacted under vacuum conditions for 1 hour.

[0032] In this embodiment, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is 1:1.

[0033] Example 2

[0034] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0035] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in a 152°C oil bath, the temperature is lowered to 137°C, and the reaction is carried out under vacuum conditions for 1 hour, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0036] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0037] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0038] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0039] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 157° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 137° C., and reacted under vacuum conditions for 1 hour.

[0040] In this embodiment, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is 3:1.

[0041] In this embodiment, after step S4, the following steps are also included:

[0042] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0043] Wherein, in step S5, the mass ratio of PCE polymer to the mixture is 0.1:1.

[0044] In step S5, the spinning solution solvent used in electrospinning is a mixture of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixture is (0.8:1.

[0045] Wherein, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0046] Among them, the parameters of the electrospinning are as follows: positive high voltage 17kv, negative high voltage 3kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 12cm, the spinning liquid propulsion speed is 0.11mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 40%.

[0047] Example 3

[0048] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0049] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in a 155°C oil bath, the temperature is lowered to 138°C, and the reaction is carried out under vacuum conditions for 1.2 hours, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0050] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0051] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0052] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0053] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 158° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 140° C., and reacted for 2 hours under vacuum conditions.

[0054] Specifically, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is (0.1-10):1.

[0055] Specifically, after step S4, the following steps are also included:

[0056] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0057] Specifically, in step S5, the mass ratio of PCE polymer to the mixture is (0.1-0.6):1.

[0058] Furthermore, in step S5, the spinning solution solvent used in electrospinning is a mixture of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixture is (0.8-0.9):1.

[0059] Furthermore, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0060] Specifically, the parameters of the electrospinning are as follows: positive high voltage 19kv, negative high voltage 5kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 22cm, the spinning liquid propulsion speed is 0.19mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 75%.

[0061] Specifically, after step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

[0062] Specifically, in step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling;

[0063] After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.

[0064] Example 4

[0065] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0066] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in a 160° C. oil bath, the temperature is lowered to 142° C., and the reaction is carried out under vacuum conditions for 1.5 hours, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0067] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0068] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0069] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0070] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 160° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 140° C., and reacted for 2 hours under vacuum conditions.

[0071] Specifically, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is 10:1.

[0072] Specifically, after step S4, the following steps are also included:

[0073] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0074] Specifically, in step S5, the mass ratio of the PCE polymer to the mixture is 0.6:1.

[0075] Furthermore, in step S5, the spinning solution solvent used in electrospinning is a mixed solution of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixed solution is 0.9:1.

[0076] Furthermore, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0077] Specifically, the parameters of the electrospinning are as follows: positive high voltage 17kv, negative high voltage 3kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 20cm, the spinning liquid propulsion speed is 0.17mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40 degrees Celsius, and the humidity range is 70%.

[0078] Specifically, after step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

[0079] Specifically, in step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling;

[0080] After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.

[0081] Example 5

[0082] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0083] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in a 158°C oil bath, the temperature is lowered to 140°C, and the reaction is carried out under vacuum conditions for 1.5 hours, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0084] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0085] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0086] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0087] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 160° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 140° C., and reacted for 2 hours under vacuum conditions.

[0088] Specifically, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is 8:1.

[0089] Specifically, after step S4, the following steps are also included:

[0090] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0091] Specifically, in step S5, the mass ratio of the PCE polymer to the mixture is 0.5:1.

[0092] Furthermore, in step S5, the spinning solution solvent used in electrospinning is a mixed solution of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixed solution is 0.8:1.

[0093] Furthermore, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0094] Specifically, the parameters of the electrospinning are as follows: positive high voltage 19kv, negative high voltage 5kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 22cm, the spinning liquid propulsion speed is 0.19mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 55%.

[0095] Specifically, after step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

[0096] Specifically, in step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling;

[0097] After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.

[0098] Example 6

[0099] A method for preparing an antimicrobial nanofiber polymer material comprises the following steps:

[0100] S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, after the reaction monomers citric acid and 1,8-octanediol are completely melted in an oil bath at 150-160°C, the temperature is lowered to 140°C, and the reaction is carried out under vacuum conditions for 1.5 hours, the reaction product is dialyzed with deionized water for 48 hours, and freeze-dried;

[0101] S2, completely dissolve 0.5 mmol of polycitrate PC in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly;

[0102] S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer;

[0103] S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

[0104] Specifically, in step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; the high-temperature melt polymerization reaction is heated to 160° C. in a nitrogen atmosphere until the monomers are melted, then cooled to 140° C., and reacted for 2 hours under vacuum conditions.

[0105] Specifically, in step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is 9:1.

[0106] Specifically, after step S4, the following steps are also included:

[0107] S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

[0108] Specifically, in step S5, the mass ratio of PCE polymer to the mixture is (0.1-0.6):1.

[0109] Furthermore, in step S5, the spinning solution solvent used in electrospinning is a mixed solution of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixed solution is 0.9:1.

[0110] Furthermore, in step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

[0111] Specifically, the parameters of the electrospinning are as follows: positive high voltage 19kv, negative high voltage 5kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 22cm, the spinning liquid propulsion speed is 0.19mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 75%.

[0112] Specifically, after step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

[0113] Specifically, in step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling;

[0114] After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.

[0115] The antimicrobial nanofiber polymer materials prepared in Examples 1 to 6 can effectively kill a variety of microorganisms including drug-resistant bacteria, and have good mechanical properties and water absorption, and good biocompatibility.

[0116] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing an antimicrobial nanofiber polymer material, characterized in that: The following steps are included: S1, taking citric acid and 1,8-octanediol in a molar ratio of 1:1 for high temperature melt polymerization, the reaction monomers citric acid and 1,8-octanediol are completely melted in an oil bath at 150-160° C., then cooled to 135-142° C., reacted under vacuum conditions for 1-1.5 hours, the reaction product was dialyzed with deionized water for 48 hours, and freeze-dried; S2. Dissolve 0.5 mmol of polycitrate PC completely in 10 mL of dimethyl sulfoxide; then add 2.5 mmol of EDC and stir evenly; then add 1 mmol of NHS and stir evenly; S3, adding antimicrobial active molecules and stirring evenly; the product was dialyzed in deionized water for 48 hours to remove unreacted poly-lysine and catalysts EDC and NHS, and freeze-dried to obtain PCE polymer; S4. After adding EDC, stir at 25°C for 30 minutes; after adding NHS, stir at 25°C for 12 hours; after adding antimicrobial active molecules, stir at 25°C for 72 hours.

2. The method for preparing an antimicrobial nanofiber polymer material according to claim 1, characterized in that: In step S1, citric acid and 1,8-octanediol are subjected to a high-temperature melt polymerization reaction in a round-bottom flask; The high temperature melt polymerization reaction is heated to 155-160°C in a nitrogen atmosphere until the monomers are melted, then cooled to 135-140°C and reacted under vacuum conditions for 1-2 hours.

3. The method for preparing an antimicrobial nanofiber polymer material according to claim 1, characterized in that: In step S3, the antimicrobial active molecule is ε-polylysine EPL, and the molar ratio of ε-polylysine EPL to polycitrate PC is (0.1-10):

1.

4. The method for preparing an antimicrobial nanofiber polymer material according to any one of claims 1 to 3, characterized in that: After step S4, the following steps are also included: S5. Add a mixture of PCE polymer and synthetic polyester polymer PE into a mixed solution of 2 mL of dichloromethane and dimethyl sulfoxide, and perform electrospinning at a voltage of 19 Kv to obtain an antimicrobial nanofiber polymer material.

5. The method for preparing an antimicrobial nanofiber polymer material according to claim 4, characterized in that: In step S5, the mass ratio of PCE polymer to the mixture is (0.1-0.6):

1.

6. The method for preparing an antimicrobial nanofiber polymer material according to claim 5, characterized in that: In step S5, the spinning solution solvent used in electrospinning is a mixed solution of dichloromethane and dimethyl sulfoxide, and the volume ratio of dichloromethane to the mixed solution is (0.8-0.9):

1.

7. The method for preparing an antimicrobial nanofiber polymer material according to claim 6, characterized in that: In step S5, the synthetic polyester polymer PE is one or a mixture of PCL, PLLA and PLGA.

8. The method for preparing an antimicrobial nanofiber polymer material according to claim 5, characterized in that: The parameters of the electrospinning are as follows: positive high voltage 5kv~19kv, negative high voltage 1kv~5kv, the needle is a No. 21 needle, the distance from the nozzle to the receiving device is 8cm~22cm, the spinning solution advancement speed is 0.1~0.19mm / min, the receiving device is a roller receiver, the receiving material is medical gauze, the receiving speed is 40rpm, the translation stroke of the push injection device is 80mm, the translation speed is 100mm / min, the temperature is room temperature to 40°C, and the humidity range is 35%~75%.

9. The method for preparing an antimicrobial nanofiber polymer material according to claim 4, characterized in that: After step S5, the method further includes step S6, characterizing the obtained antimicrobial nanofiber polymer material once before sampling and once after sampling.

10. The method for preparing an antimicrobial nanofiber polymer material according to claim 9, characterized in that: In step S6, the characterization method includes scanning electron microscopy, XRD, BET, and electrochemistry before sampling; After sampling, it includes scanning electron microscopy, XRD, electrochemistry, fluorescence spectrophotometer, Fourier transform infrared spectroscopy, and ultraviolet spectrophotometer.