Preparation method of super-hydrophobic fabric for anti-icing, optical / electric heating and electromagnetic induction heat deicing

By using chemical oxidation polymerization and spraying technology to prepare polypyrrole and ferric oxide particle layers on polyester fabrics, and using PDMS solution for hydrophobic modification, the anti-icing and multiple thermal conversion de-icing functions of the fabric were achieved, solving the problem that the fabric is easy to Freezing issues, improved safety and durability.

CN118854677AInactive Publication Date: 2024-10-29TIANJIN POLYTECHNIC UNIV

Patent Information

Application Number
CN202410883483.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to implement anti-icing and multiple thermal conversion de-icing functions on fabrics with existing technology. Especially in outdoor activities and transportation, fabrics are prone to freezing, affecting safety and comfort.

Method used

Chemical oxidation polymerization and spraying technology are used to prepare polypyrrole and ferroferric oxide particle layers on the surface of polyester fabrics, and PDMS solution is used for hydrophobic modification, combining photothermal, electric heating and electromagnetic induction thermal effects to achieve passive anti-icing and active self-heating removal. Ice function.

Benefits of technology

The prepared superhydrophobic fabric has good hydrophobic effect, photothermal, electric heating and electromagnetic induction thermal properties, can effectively prevent freezing and quickly remove ice, and improves safety and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854677A_ABST
    Figure CN118854677A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-hydrophobic fabric for anti-icing, optical / electric heating and electromagnetic induction heat deicing, which adopts simple methods of chemical oxidative polymerization, spraying and soaking to prepare a coating with anti-icing, optical / electric heating and electromagnetic induction heat deicing functions on the surface of a polyester fabric. According to the present invention, the selected polypyrrole preparation process is mature, the Fe3O4 is easy to obtain and has the low price, the experimental methods comprise oxidative polymerization, spraying and soaking, the operation process is simple, the experiment is easy to reproduce, the environmental-friendly PDMS is adopted to perform the surface material modification, and the preparation method is simple and easy to operate; the anti-icing and deicing device is suitable for the field of anti-icing and deicing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a super-hydrophobic fabric for anti-icing, photothermal, electrothermal and electromagnetic induction thermal deicing, and belongs to the application field of super-hydrophobic fabrics with photothermal, electrothermal and electromagnetic induction thermal effects. Background Art

[0002] Ice is a common natural phenomenon, but its accumulation can have adverse effects on roads, aircraft, power lines, special work clothes, etc. in transportation, outdoor activities and daily life. For example, fabrics are prone to ice formation in rainy and snowy weather, which not only makes the clothing stiff and heavy, but also reduces the wearer's freedom of movement and comfort. Similarly, tents and other outdoor equipment may also be at risk of damage under the weight of ice and snow. Therefore, the development of new fabrics that can resist ice formation and have all-weather deicing functions is of great significance to improve safety, durability and comfort. The development of such fabrics will provide better protection for outdoor activities while reducing maintenance costs and potential risks caused by ice formation.

[0003] For example, Chinese patent CN115160857 B discloses "a super-hydrophobic anti-icing coating for passive photothermal deicing and its preparation method and application", which mainly pours ethyl cellulose, hollow porous carbon fibers derived from ZIF-8 and sodium chloride into anhydrous ethanol in sequence, and after ultrasonication and stirring, sprays them on the surface of the substrate as the bottom layer. After the bottom layer is naturally dried and solidified, pour fluorinated silicon dioxide into ethyl acetate and stir, spray it on the bottom layer as the surface layer, and then wait for the surface layer to dry and solidify naturally to obtain the coating. The coating has both good anti-icing performance and excellent rapid deicing effect, providing double insurance against ice damage. For example, Chinese patent CN 116815495A discloses a method for preparing a super-hydrophobic fabric for anti-icing and photo-thermal deicing. First, the fabric is pretreated, then immersed in an activation solution to obtain an activated nickel layer, then immersed in a plating solution to plate copper and nickel on the surface, and finally a layer of PDMS solution is evenly sprayed on the surface to obtain a super-hydrophobic fabric for anti-icing and photo-thermal deicing, which has both photo-thermal and electro-thermal deicing functions.

[0004] Therefore, polymer polypyrrole and ferroferric oxide particles are used as photothermal and electrothermal conversion materials. At the same time, ferroferric oxide particles give the fabric electromagnetic induction thermal properties. PDMS (polydimethylsiloxane) is used as a surface modification material to simply prepare a super hydrophobic fabric for anti-icing, photo / electrothermal and electromagnetic induction thermal deicing. A deicing fabric with anti-icing and triple thermal conversion mode can be prepared. A layer of polypyrrole is wrapped on the surface of the fabric by chemical oxidation polymerization to improve the photo / electrothermal performance and surface roughness of the fabric, and then ferroferric oxide particles are sprayed to further improve the photo / electrothermal performance of the fabric while improving its surface roughness. The most important thing is that ferroferric oxide particles give the fabric certain electromagnetic induction thermal properties. Finally, PDMS solution is sprayed on the surface of the fabric to modify its hydrophobicity. The prepared photo / electrothermal and electromagnetic induction thermal super hydrophobic materials effectively give polyester fabrics the ability to prevent icing and deicing. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a super-hydrophobic fabric for anti-icing, photo- / electro-thermal and electromagnetic induction thermal deicing, and to prepare a coating with anti-icing, photo- / electro-thermal and electromagnetic induction thermal deicing on the surface of a polyester fabric by a simple method of chemical oxidation polymerization and spraying, so as to achieve the effects of passive anti-icing and active self-heating deicing, and enrich the existing deicing methods of self-heating fabrics.

[0006] The technical solution of the present invention is:

[0007] Step 1: prepare a pretreatment solution by preparing a NaOH solution of a certain concentration at room temperature;

[0008] Step 2: Prepare an oxidative polymerization solution by adding pyrrole monomer and hydrochloric acid in a certain proportion to deionized water to obtain solution A. Similarly, add ferric chloride and hydrochloric acid in a certain proportion to deionized water to obtain solution B. Finally, mix solutions A and B to obtain an oxidative polymerization solution.

[0009] Step 3: prepare a Fe3O4 mixed solution. Add Fe3O4 nanoparticles to a sodium alginate aqueous solution with a certain mass fraction and stir the mixture in a water bath to obtain a Fe3O4 mixed solution.

[0010] Step 4: Prepare a PDMS solution by mixing silica gel and silica gel curing agent in a certain ratio, adding n-hexane to dilute, and treating with magnetic stirring and ultrasound to obtain a uniformly dispersed PDMS solution.

[0011] Step 5: Prepare photo / electrothermal and electromagnetic induction thermal super-hydrophobic fabrics. First, pretreat the polyester fabric with the above-mentioned NaOH solution, then immerse the fabric in the above-mentioned oxidative polymerization solution for polymerization reaction, then spray a certain volume of Fe3O4 mixed solution on the surface of the fabric, and finally immerse the fabric in the above-prepared PDMS solution to obtain photo / electrothermal and electromagnetic induction thermal super-hydrophobic fabrics.

[0012] Furthermore, the mass / volume concentration of the NaOH solution prepared in step 1 is 50-100 g / L.

[0013] Furthermore, in the oxidative polymerization solution in step 2, the concentration of pyrrole monomer and hydrochloric acid in solution A is 0.5-1.5 mol / L, and the ratio of the two is 1:0.5-1.5. The concentration of ferric chloride in solution B is 1.5-2.5 mol / L, and the concentration of hydrochloric acid is 0.5-1.5 mol / L, and the ratio of the two is 1:0.5-1.5. The concentration ratio of pyrrole monomer and ferric chloride is 1:2.

[0014] Furthermore, in the preparation of the Fe3O4 solution described in step three, the mass fraction of the sodium alginate aqueous solution is 0.1-0.5%, the concentration of the Fe3O4 solution is 0.1 mol / L, the water bath temperature is 80°C, and the stirring time is greater than 1 h.

[0015] Furthermore, in the preparation of the PDMS solution described in step 4, the mass ratio of silica gel to silica gel curing agent is 10:1, and the magnetic stirring and ultrasonic treatment time are both greater than 30 minutes.

[0016] Furthermore, in step five, a photo / electro-thermal and electromagnetic induction thermal super-hydrophobic fabric is prepared by a simple method of oxidative polymerization reaction and spraying. The specific steps are as follows: a polyester fabric of a certain size is immersed in a NaOH pretreatment solution to clean impurities, and after deionized water washing, it is dried in an oven at 80°C for more than 1 hour. Then the pretreated polyester fabric is immersed in an oxidative polymerization solution for polymerization under low temperature conditions for more than 6 hours. After the reaction is completed, it is washed with deionized water and dried to obtain a polyester fabric with a layer of polypyrrole deposited. Secondly, 0.5 to 2 mL of Fe3O4 mixed solution is sprayed on the surface of the fabric, and it is cured and dried in an oven at 80°C for more than 0.5 hours. Finally, the fabric is immersed in a PDMS solution for 2 to 60 seconds and cured in an oven at 80°C for more than 1 hour to obtain a super-hydrophobic fabric for anti-icing, photo / electro-thermal and electromagnetic induction thermal deicing.

[0017] The advantages of the present invention are:

[0018] The selected polypyrrole preparation process is mature, and Fe3O4 is easy to obtain and cheap. The experimental method uses oxidative polymerization and spraying, the operation process is simple, and the experiment is easy to reproduce. The environmentally friendly PDMS is used for surface modification materials, which is more green and environmentally friendly.

[0019] The contact angle of the fabric prepared by this method is 152°, which has a good hydrophobic effect. It can reach 74.3°C under the illumination intensity of 1 sun, and has good photothermal conversion performance. When a voltage of 10V is applied on both sides of the fabric, it can quickly reach an equilibrium temperature of 72.2°C, and has good electrothermal conversion performance. The fabric can reach a maximum temperature of 71.4°C in just 5 minutes on an electromagnetic induction heating coil with a voltage of 8V, and has good electromagnetic induction thermal performance. The excellent hydrophobic effect gives the fabric passive anti-icing skills, and the excellent thermal conversion ability enables its surface to complete the task of active deicing. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor.

[0021] Figure 1 This is a surface SEM image of a super-hydrophobic fabric for anti-icing, photo-thermal / electrical-thermal and electromagnetic-induction thermal deicing prepared in Example 1;

[0022] Figure 2 is the surface SEM image of untreated polyester fabric;

[0023] Figure 3 This is a surface SEM image of the polypyrrole polyester fabric prepared in Comparative Example 1;

[0024] Figure 4 This is a surface SEM image of the Fe3O4 / polypyrrole polyester fabric prepared in Comparative Example 2;

[0025] Figure 5 The super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1, the untreated polyester fabric and the fabrics prepared in Comparative Examples 1 and 2 were subjected to 1000 W / m 2 Temperature variation curve under light intensity;

[0026] Figure 6 The temperature variation curves of a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1, an untreated polyester fabric, and fabrics prepared in Comparative Examples 1 and 2 when a voltage of 10 V is applied on both sides;

[0027] Figure 7The temperature variation curves of the super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction thermal deicing prepared in Example 1, the untreated polyester fabric, and the fabrics prepared in Comparative Examples 1 and 2 on an electromagnetic induction heating coil with a voltage of 8V;

[0028] Figure 8 A comparison diagram of the surface contact angles of a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction thermal deicing prepared in Example 1, an untreated polyester fabric, and fabrics prepared in Comparative Examples 1 and 2;

[0029] Fig. 9 A comparison chart of the surface icing time and surface ice adhesion strength of a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1, an untreated polyester fabric, and fabrics prepared in Comparative Examples 1 and 2;

[0030] Fig.10 This is a comparison chart of the time required to melt ice particles using photothermal / electrical heating and electromagnetic induction heating of a superhydrophobic fabric prepared in Example 1 for anti-icing, photothermal / electrical heating and electromagnetic induction heating deicing. DETAILED DESCRIPTION

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical scheme of the present invention is further described below in conjunction with the accompanying drawings, embodiments and comparative examples. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0032] First, the "embodiment 1" referred to herein refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. Secondly, the present invention is described in detail using a structural schematic diagram, etc. When describing the embodiment of the present invention in detail, for the sake of convenience, the schematic diagram will not be partially enlarged according to the general proportion, and the schematic diagram is only an example, which should not limit the scope of protection of the present invention. In addition, in actual production, a three-dimensional space of length, width and depth should be included.

[0033] In addition, the abbreviations mentioned in the present invention are all fixed abbreviations in the art, and some of the abbreviations are explained as follows: PET: polyester fabric; PDMS: polydimethylsiloxane; PPy: polypyrrole; SEM: scanning electron microscope.

[0034] Embodiment 1

[0035] This embodiment prepares a super hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction thermal deicing according to the following steps;

[0036] Step 1: Prepare the pretreatment solution NaOH solution

[0037] Slowly add NaOH particles into deionized water to prepare 100 mL of NaOH pretreatment solution with a mass / volume concentration of 70 g / L;

[0038] Step 2: Preparation of oxidative polymerization solution

[0039] First, pyrrole monomer and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.1 mol / L pyrrole and 0.1 mol / L hydrochloric acid. Similarly, ferric chloride and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.2 mol / L ferric chloride and 0.1 mol / L hydrochloric acid.

[0040] Step 3: Prepare Fe3O4 mixed solution

[0041] Fe3O4 nanoparticles were added to a 0.2% by mass sodium alginate aqueous solution and stirred in a water bath at 80°C for 1 hour to prepare a 0.1 mol / L Fe3O4 solution.

[0042] Step 4: Prepare PDMS solution

[0043] The silica gel prepolymer and the curing agent were mixed in a mass ratio of 10:1 and diluted with n-hexane to obtain 50 mL of PDMS solution.

[0044] Step 5: Preparation of photo- / electro-thermal and electromagnetic induction thermal super-hydrophobic fabrics

[0045] The polyester fabric was cut into 5×5cm specifications, immersed in the NaOH pretreatment solution for ultrasonic treatment for 1h, washed with deionized water and dried. Secondly, the treated fabric was immersed in the oxidative polymerization solution composed of A and B above, placed in a refrigerator for low-temperature polymerization for 6h, taken out, washed with deionized water and dried in an oven to form a polypyrrole layer on the fabric surface. Then the fabric was fixed on a flat plate, 1mL of Fe3O4 mixed solution was sprayed on the fabric surface with an automatic spray gun, placed in an 80℃ oven for drying for 0.5h, and a Fe3O4 particle layer was formed on the fabric surface. Finally, the fabric was immersed in the PDMS solution for 3s and placed in an 80℃ oven for curing for 1h to obtain a photo / electrothermal and electromagnetic induction thermal superhydrophobic fabric.

[0046] The surface condition of the super-hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in this embodiment can be found in Figure 1 , Figure 1 The surface SEM image of the fabric prepared in Example 1 of the present invention is shown in FIG. Figure 1 As shown, the surface of the polyester fabric treated with oxidative polymerization, spray coating and immersion PDMS is loaded with a large amount of uniform coating material.

[0047] Comparative Example 1

[0048] In this comparative scheme, a polyester fabric with polypyrrole loaded on its surface is prepared according to the following steps.

[0049] Step 1: Prepare the pretreatment solution NaOH solution

[0050] Slowly add NaOH pellets into deionized water to prepare a NaOH pretreatment solution with a mass of 100 mL and a volume concentration of 70 g / L;

[0051] Step 2: Preparation of oxidative polymerization solution

[0052] First, pyrrole monomer and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.1 mol / L pyrrole and 0.1 mol / L hydrochloric acid. Similarly, ferric chloride and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.2 mol / L ferric chloride and 0.1 mol / L hydrochloric acid.

[0053] Step 3: Preparation of polyester fabric with polypyrrole loaded on the surface

[0054] The polyester fabric was cut into 5×5 cm specifications, immersed in the NaOH pretreatment solution for ultrasonic treatment for 1 hour, washed with deionized water and dried. Then, the treated fabric was immersed in the oxidative polymerization solution composed of A and B, placed in a refrigerator for low-temperature polymerization for 6 hours, then taken out, washed with deionized water and dried in an oven to obtain a polyester fabric loaded with polypyrrole on the surface.

[0055] For the surface condition of the polyester fabric loaded with polypyrrole prepared in this comparative example, please refer to Figure 3 , Figure 3 This is a surface SEM image of the fabric prepared in Comparative Example 1 of the present invention. Figure 3 As shown, a polypyrrole film is formed on the surface of the fabric after oxidative polymerization.

[0056] Comparative Example 2

[0057] In this comparative scheme, a polyester fabric with surface loaded polypyrrole and Fe3O4 particles is prepared according to the following steps.

[0058] Step 1: Prepare the pretreatment solution NaOH solution

[0059] Slowly add NaOH particles into deionized water to prepare 100 mL of NaOH pretreatment solution with a mass / volume concentration of 70 g / L;

[0060] Step 2: Preparation of oxidative polymerization solution

[0061] First, pyrrole monomer and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.1 mol / L pyrrole and 0.1 mol / L hydrochloric acid. Similarly, ferric chloride and hydrochloric acid are slowly added into deionized water to obtain a mixed solution of 0.2 mol / L ferric chloride and 0.1 mol / L hydrochloric acid.

[0062] Step 3: Prepare Fe3O4 mixed solution

[0063] Fe3O4 nanoparticles were added to a 0.2% by mass aqueous solution of sodium alginate and stirred in a water bath at 80°C for 1 h to prepare a 0.1 mol / L Fe3O4 solution.

[0064] Step 4: Preparation of polyester fabric with surface loaded polypyrrole and Fe3O4 particles

[0065] The polyester fabric was cut into 5×5cm specifications, immersed in the NaOH pretreatment solution for ultrasonic treatment for 1h, washed with deionized water and dried. Secondly, the treated fabric was immersed in the oxidative polymerization solution composed of A and B above, placed in a refrigerator for low-temperature polymerization for 6h, then taken out, washed with deionized water and dried in an oven to form a polypyrrole layer on the fabric surface. Then the fabric was fixed on a flat plate, 1mL of the Fe3O4 mixed solution was sprayed on the fabric surface with an automatic spray gun, and placed in an 80℃ oven for drying for 0.5h to obtain Fe3O4 particles on the fabric surface, and finally a polyester fabric with polypyrrole and Fe3O4 particles loaded on the surface was obtained.

[0066] For the surface condition of the polyester fabric loaded with polypyrrole and Fe3O4 particles prepared in this comparative example, please refer to Figure 4 , Figure 4 This is a surface SEM image of the fabric prepared in Comparative Example 2 of the present invention. Figure 4 As shown, a layer of polypyrrole film and Fe3O4 particle layer were formed on the surface of the fabric after oxidative polymerization and spraying treatment.

[0067] See also Figure 5 , Figure 5 The temperature change curves of the super-hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction thermal deicing prepared in Example 1 and the original polyester fabric, and the fabrics prepared in Comparative Example 1 and Comparative Example 2 under the illumination intensity of 1 sun. It can be seen from the figure that the surface equilibrium temperature of the super-hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction thermal deicing prepared can reach 74.3°C, and it has good photothermal conversion performance.

[0068] See also Figure 6 , Figure 6The temperature change curves of a super-hydrophobic fabric for anti-icing, photo / electro-thermal and electromagnetic induction thermal deicing prepared in Example 1 and the original polyester fabric, and the fabrics prepared in Comparative Example 1 and Comparative Example 2 when a voltage of 10V is applied on both sides of the sample. It can be seen from the figure that the surface equilibrium temperature of the super-hydrophobic fabric for anti-icing, photo / electro-thermal and electromagnetic induction thermal deicing prepared can reach 72.2°C, and it has excellent electrothermal conversion performance.

[0069] See also Figure 7 , Figure 7 The temperature change curves of the super-hydrophobic fabric for anti-icing, photo- / electric-heating and electromagnetic induction thermal deicing prepared in Example 1 and the original polyester fabric, and the fabrics prepared in Comparative Example 1 and Comparative Example 2 when an electromagnetic induction heating coil with a voltage of 8V is applied on both sides of the sample. It can be seen from the figure that the surface temperature of the super-hydrophobic fabric for anti-icing, photo- / electric-heating and electromagnetic induction thermal deicing prepared can reach 71.4°C, and it has excellent electromagnetic induction thermal performance.

[0070] See also Figure 8 , Figure 8 The surface wettability comparison diagram of a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1, an original polyester fabric, a fabric prepared in Comparative Example 1 and a fabric prepared in Comparative Example 2 is shown in FIG. Figure 8 It can be seen that the static contact angle of the super hydrophobic surface prepared in this embodiment 1 is 152°, which has an excellent hydrophobic effect.

[0071] See also Fig. 9 , Fig. 9 The medium dark group is a comparison chart of the freezing time of the super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1 and the fabric surface prepared in Comparative Example 1. 10 μL of water is dropped on the fabric surface prepared in Example 1 and Comparative Example 1, respectively. Fig. 9 As shown in the figure, under the same conditions, the fabric prepared in Example 1 has a longer freezing time and has good anti-icing performance. The light-colored group is a comparison of the ice adhesion strength of the super-hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing prepared in Example 1 and the original polyester fabric, and the fabrics prepared in Comparative Example 1 and Comparative Example 2. Fig. 9 As shown, the fabric prepared in Example 1 has lower ice adhesion strength and good ice-repelling performance.

[0072] See also Fig.10 , Fig.10This is a comparison chart of the melting time of ice particles on the electromagnetic induction heating coils with 10V and 8V voltages applied on both sides of the super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heating deicing prepared in Example 1 under the illumination intensity of one sun. Ice particles formed by 10μL water droplets were placed on the surface of the fabric, and deicing experiments were carried out in an environment of -5℃ using three heating methods, such as Fig.10 As shown, it only takes 209s, 137s and 181s for the ice on the surface of the fabric prepared in Example 1 to melt into liquid water, indicating that the fabric prepared in Example 1 has good deicing properties of photothermal / electrical heating and electromagnetic induction heating.

[0073] In summary, the present invention discloses a method for preparing a super-hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction thermal deicing. The method has high feasibility, mild preparation conditions, simple and easy process, is suitable for large-scale preparation and application, can be applied to outdoor tents, etc., and is also suitable for industrial fields such as anti-icing and deicing.

[0074] It should be noted that the above embodiments and comparative examples are only used to illustrate the technical solutions of the present invention, rather than to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing, characterized in that: The method comprises the following steps: firstly, pretreating polyester fabric with NaOH solution, then immersing the fabric in pyrrole oxidative polymerization solution for polymerization reaction, polymerizing a layer of polypyrrole on its surface, secondly, spraying a certain volume of mixed solution containing Fe3O4 particles uniformly on the fabric surface, and finally immersing the fabric in polydimethylsiloxane (PDMS) solution, taking it out and drying and curing it in an oven, so as to obtain a super hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction thermal deicing.

2. The method for preparing a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing according to claim 1, characterized in that: The mass / volume concentration of the NaOH solution is 50-100 g / L, and the polyester fabric is immersed in the NaOH solution for pretreatment for 1-2 hours.

3. The method for preparing a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing according to claim 1, characterized in that: The oxidative polymerization solution of pyrrole is composed of pyrrole monomer, ferric chloride and hydrochloric acid, wherein the concentration of pyrrole monomer is 0.5-1.5 mol / L, the concentration of ferric chloride is 1.5-2.5 mol / L, the concentration of hydrochloric acid is 1.0-3.0 mol / L, and the ratio of the three concentrations is 1:(1-3):(1-3). The polymerization time of the reaction experiment is 6-12 h, and the polymerization temperature is -15-5°C.

4. The method for preparing a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing according to claim 1, characterized in that: A mixed solution containing Fe3O4 particles, in which the mass fraction of sodium alginate is 0.1-0.5% and the concentration of Fe3O4 is 0.1 mol / L, is sprayed on 25 cm 2 Fabrics of different sizes require 0.5 to 3 mL of Fe3O4 mixed solution.

5. The method for preparing a super hydrophobic fabric for anti-icing, light / electric heating and electromagnetic induction heat deicing according to claim 1, characterized in that: The mass ratio of silica gel to silica gel curing agent in the polydimethylsiloxane (PDMS) solution is 10:1, the immersion time is 2 to 60 seconds, and the drying and curing temperature is 40 to 110°C.

6. A super hydrophobic fabric for anti-icing, photo / electric heating and electromagnetic induction heat deicing prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The selected base fabric is not limited to polyester fabric, and should include other fabrics such as natural fiber fabric and chemical fiber fabric that will not be damaged when immersed in a weakly acidic pyrrole oxidation solution. The prepared fabric is specifically used in the field of anti-icing and deicing.

Citation Information

Patent Citations

  • Photo-thermal deicing surface coating and preparation method thereof

    CN111518474A

  • Preparation method of super-hydrophobic fabric for icing prevention and photo-thermal deicing

    CN115161992A

  • Preparation method of soft elastic super-hydrophobic low-ice adhesion surface with photothermal effect

    CN115260897A

  • Anti-icing coating for power transmission line and preparation method of anti-icing coating

    CN115595023A

  • Photo-thermal super-hydrophobic anti-icing and deicing coating and preparation method thereof

    CN116376414A

Cited By

  • Self-cleaning sensing type composite coating for fabric and preparation method of self-cleaning sensing type composite coating

    CN119265941A