A HDPE water supply and drainage plastic pipe system for dredging

By using high-temperature water activation technology combined with HDPE material and nano-copper catalyst in the water supply and drainage pipeline, the problems of low efficiency and insufficient safety of existing cleaning methods are solved, and rapid and thorough dirt removal and pipeline cleaning are achieved, which extends the Pipe lifespan.

CN118856113BActive Publication Date: 2024-12-06ZHEJIANG AKAN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411332323.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

The existing water supply and drainage pipe cleaning methods have problems such as low efficiency, insufficient safety, hazards to the human body, and incomplete treatment of dirt. We seek a more convenient, safe, efficient and time-saving cleaning system.

Method used

The HDPE water supply and drainage plastic pipeline system is used, and the inner layer is composed of HDPE, biodegradable materials, lubricants and nano-copper catalysts. The nano-copper catalyst is activated through high-temperature water, decomposes and dissolves the dirt in the pipeline, and rushes out with the water flow to complete cleaning.

Benefits of technology

It achieves rapid and thorough pipeline cleaning, reduces the need for manual effort, ensures the cleanliness of dirt treatment, and extends the service life of the pipeline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118856113B_ABST
    Figure CN118856113B_ABST
Patent Text Reader

Abstract

The invention relates to a HDPE water supply and drainage plastic pipe system for dredging, comprising an active inner layer and a temperature-resistant outer layer, wherein the temperature-resistant outer layer is a performance supporting layer, the active inner layer is a main degradation active layer, and the temperature-resistant outer layer serves as a performance supporting protective layer for the active inner layer; the active inner layer comprises HDPE and biodegradable materials, a lubricant and a nano copper catalyst, and can be applied to the dredging of water supply and drainage plastic pipes, and has excellent prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of drainage pipes, and in particular to the field of a HDPE water supply and drainage plastic pipe system for dredging. Background Art

[0002] At present, there are two main ways to clean the inside of water supply and drainage pipes: one is the physical cleaning method, which uses special tools or pipe cleaning robots to clean the pipes. However, using special tools for cleaning requires a lot of manpower and time, and is very inefficient and labor-intensive; although the pipe cleaning robot has excellent efficiency and cleaning quality, it can autonomously select the most suitable tools and strategies for cleaning operations according to the size and degree of blockage of the pipe. Compared with traditional manual dredging, the robot does not require manpower input, is not restricted by the working environment and time, and can improve the dredging efficiency, but there are also many problems: Robot pipeline technology has certain challenges in terms of safety and usage restrictions. Although the robot has autonomous navigation capabilities, the risk of collision and blockage still exists in complex pipeline environments; in addition, due to the complex environment of some pipelines and the presence of special impurities, the robot may be restricted and unable to successfully complete the dredging task.

[0003] Another cleaning method is chemical cleaning, which usually refers to the use of chemical solvents to dissolve the dirt in the pipe, including strong alkali cleaning, strong acid cleaning, descaling agent cleaning, or weaker acidic and alkaline chemical reagents to neutralize the dirt or naturally fall off after chemical reaction. The former cleans quickly and has obvious effects, but because it uses detergents, if the dosage is improper, it is easy to corrode the pipes, and neutralization measures must be taken after use. In addition, detergents are dangerous to the human body, and accidental contact will cause serious consequences; the latter saves time and effort, but it takes a long time and does not handle the dirt thoroughly and cleanly enough.

[0004] Therefore, it is very important to find a more convenient, safe, efficient, time-saving and labor-saving pipeline structure system that is conducive to pipeline cleaning. Summary of the invention

[0005] The technical purpose of the present invention is to solve the problems in the background technology and provide a HDPE water supply and drainage plastic pipe system for dredging.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] A HDPE plastic water supply and drainage pipe system for dredging, the HDPE plastic water supply and drainage pipe for dredging comprising an active inner layer and a temperature-resistant outer layer, the temperature-resistant outer layer being a performance supporting layer, the active inner layer being a main degradation active layer, and the temperature-resistant outer layer being a performance supporting protective layer for the active inner layer; the active inner layer comprising HDPE and biodegradable materials, a lubricant and a nano copper catalyst, the thickness of the active inner layer and the wall thickness of the temperature-resistant outer layer being in a ratio ranging from (1:6) to (1:19).

[0008] When the pipeline dredging function is played, high-temperature water is passed into the water supply and drainage pipe for soaking. The water temperature is controlled at 60-90°C and the soaking time is 1-48 hours. The nano-copper catalyst is activated by high temperature to decompose the inner layer material. The degraded internal dirt and the inner layer material can be dissolved in the sewage and stripped off by water, and flushed out of the pipeline with the water flow, completing the dredging process. Specifically, the water temperature of the high-temperature water, the formula of the inner layer pipe and the wall thickness of the pipe are adjusted accordingly according to the actual usage scenario.

[0009] Preferably, the raw materials of the inner layer include 30-60 parts of HDPE high-density polyethylene resin, 5-20 parts of linear low-density polyethylene, 5-10 parts of polybutylene adipate / terephthalate PBAT, 5-10 parts of polylactic acid PLA, 5-10 parts of polyhydroxyalkanoate PHA, and 0.5-10 parts of nano copper. The lubricant includes fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 0.5-2 parts, calcium stearate is 1-8 parts, and zinc stearate is 1-8 parts, and all parts are by mass, wherein the mass parts are not limited to 100 parts.

[0010] As a further preference, HDPE high-density polyethylene resin is 48 parts, linear low-density polyethylene is 14 parts, polybutylene adipate / terephthalate PBAT is 8 parts, polylactic acid PLA is 6 parts, polyhydroxyalkanoate PHA is 7 parts, nano copper is 6 parts, and the lubricant includes fluorinated polymer PPA, calcium stearate and zinc stearate, wherein the fluorinated polymer PPA is 1.2 parts, calcium stearate is 4.2 parts, and zinc stearate is 4.2 parts.

[0011] The invention has the advantage of selecting HDPE high-density polyethylene resin as the main component. HDPE is a highly crystalline, non-polar thermoplastic resin with good heat resistance and cold resistance, good chemical stability, high rigidity and toughness, good mechanical strength, and good dielectric properties and environmental stress cracking resistance.

[0012] The invention has the advantages that a small amount of linear low-density polyethylene is added to make up for the tensile strength, penetration resistance, tear resistance and elongation of the HDPE resin pipe alone; in addition, polybutylene adipate / terephthalate PBAT, polylactic acid PLA, polyhydroxyalkanoate PHA and lubricant are added, polybutylene adipate / terephthalate PBAT has good ductility and elongation at break, as well as good heat resistance and impact resistance; in addition, it has excellent biodegradability and is one of the most popular biodegradable materials in the research of biodegradable plastics and the best market application; polylactic acid PLA is a new type of biodegradable material with good thermal stability and good solvent resistance, and can be processed in a variety of ways, such as extrusion, spinning, biaxial stretching, injection blow molding, etc. In addition to being biodegradable, the products made of polylactic acid have good biocompatibility, glossiness, transparency, hand feel and heat resistance; polyhydroxyalkanoate PHA It is a kind of outstanding biodegradable polyester found in nature. PHA has the characteristics of material variability, nonlinear optical properties, piezoelectric properties, gas barrier properties, thermoplasticity, biodegradability, good biocompatibility, etc. It is applied to the production of the inner layer of the pipeline of the present invention and has good application prospects; fluorine-containing polymer PPA, calcium stearate, and zinc stearate are used as lubricant additives, which have higher stability.

[0013] The invention has the advantage that copper-based nanocatalysts are widely used in organic synthesis, electrocatalysis and photocatalysis in the field of catalysis. Compared with noble metals such as gold and silver, copper deposits are abundant, mining costs are low, and a variety of methods for preparing copper-based nanomaterials are practical and direct. Copper nanomaterials are particularly attractive, with stable physical and chemical properties, and are easy to load on polymer material framework carriers. Nano-copper is activated as a catalyst for degrading dirt inside the pipeline. Under high temperature (60-90°C), the nano-copper catalyst is activated, the inner layer material decomposes and degrades the dirt inside the pipeline, and then the decomposed inner layer is gradually detached, and then the dirt adhering to the inner layer is separated together with the sewage, thereby achieving the purpose of cleaning. In this process, only high-temperature water needs to be passed into the pipeline, soaked for a predetermined time, and then the sewage is discharged to completely clear the dirt attached to the inside of the pipeline, without the need for additional manual effort, and it is cleaned immediately after flushing, which is convenient, fast and efficient.

[0014] The advantage of the present invention is that nano copper is used as a catalyst for degrading the dirt in the pipeline, and the above-mentioned biodegradable material is used as a skeleton, so that the degradation effect can be significantly improved.

[0015] A HDPE plastic pipe for water supply and drainage for dredging, the production of which includes the following process steps:

[0016] Step S1: preparing the raw materials for the inner layer of the water supply and drainage pipe: premixing HDPE high-density polyethylene resin, linear low-density polyethylene resin, polybutylene adipate / terephthalate PBAT, polylactic acid PLA, polyhydroxyalkanoate PHA, fluorine-containing polymer PPA, lubricant and nano copper in a suitable proportion and then melt-granulating for standby use;

[0017] Step S2: preparing the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: preparing reduced graphene oxide and PE-RT high-temperature resistant polyethylene, mixing them in proportion, and then melting and granulating them for later use;

[0018] Step S3: co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure inside the tube.

[0019] As a further preference, the raw materials of step S1 further include vinyltrimethoxysilane and nano-silicon dioxide nSiO2, and vinyltrimethoxysilane is used as a carrier to load the nano-silicon dioxide nSiO2; the mass fractions of vinyltrimethoxysilane and nano-silicon dioxide are 0.05-0.1 parts and 5-10 parts respectively.

[0020] The invention has the advantage that nano silicon dioxide nSiO2 is mixed into HDPE by using vinyl trimethoxysilane as a carrier for co-extrusion, which can improve the bending strength and impact strength of the composite material and enhance the anti-creep performance of the pipeline.

[0021] Preferably, the preparation process of reduced graphene oxide in step S2 is to first preliminarily prepare graphene oxide with graphite oxide attached by Hummers method, pickle the prepared graphene oxide with 3% H2SO4 solution and 0.5% H2O2 solution for 20-28h, and then wash it with the same acid solution for multiple times to remove part of the graphite oxide, and the number of washing times is 10-15 times; the pickled graphene oxide is dried at 90-105°C to a constant weight, then resuspended and ultrasonicated for 24h to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 80-150 seconds to obtain reduced graphene oxide rGO.

[0022] Preferably, in step S2, the total mass fraction of reduced graphene oxide and PE-RT high temperature resistant polyethylene is 100 parts; the mass fraction of reduced graphene oxide is 1-5 parts, and the rest is PE-RT high temperature resistant polyethylene.

[0023] The advantage of adopting the present invention is that reduced graphene oxide (rGO) has excellent mechanical properties and has broad application prospects in polymer-based nanocomposites. Adding reduced graphene oxide rGO to the preparation of pipelines can significantly improve various mechanical properties of the material, such as tensile properties, impact resistance, hardness, tensile strength, etc., and can also improve the anti-aging performance of the pipeline and extend the service life of the pipeline.

[0024] Preferably, in step S3, the functional inner layer plastic pellets and the heat-resistant outer layer plastic pellets obtained in step S1 and step S2 are formed by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the functional inner layer is 140-160°C; the extrusion temperature of the heat-resistant outer layer is 165-185°C.

[0025] The invention has the advantage of co-extruding the active inner layer and the temperature-resistant outer layer to prepare the HDPE water supply and drainage plastic pipe, which can prevent the outer layer from being affected when the inner layer degrades the dirt, thereby reducing or failing the pipe cleaning effect.

[0026] Preferably, the outer side of the heat-resistant outer layer is fixedly covered with protective cotton, the protective cotton is made of high-temperature resistant material, the outer side of the protective cotton is fixedly installed with a pipeline shell, the outer side of the heat-resistant outer layer is also fixedly installed with a movable rod, the top of the movable rod is fixedly installed with a fixed plate, and the movable rod is made of a telescopic structure;

[0027] The functional inner layer and the heat-resistant outer layer are arranged at the innermost circle of the pipeline, a limiting spring is fixedly installed on the outer side of the heat-resistant outer layer, the top end of the limiting spring is fixedly connected to the inner side of the pipeline shell, and the pipeline shell is made of elastic material; the limiting spring is sleeved on the outer side of the movable rod;

[0028] A stabilizing spring is fixedly installed on the top of the fixing plate, and an elastic protective pad is fixedly installed on the top of the stabilizing spring.

[0029] The advantage of adopting the present invention is that through the specific pipeline structure setting, protective cotton is also arranged outside the temperature-resistant outer layer. The protective cotton is also made of high-temperature resistant material, which can protect the inner layer and prevent the inner layer from being damaged by the external high-temperature environment, thereby extending the service life of the drainage pipe fittings.

[0030] The advantage of adopting the present invention is that through the design of the limiting spring, the movable rod, the pipe shell and the protective cotton, when the pipe is installed, the pipe shell can be contracted through the contraction of the movable rod, thereby causing the limiting spring to contract, so that the drain pipe can be firmly installed in the channel; and the design of the stabilizing spring leaf and the protective pad protects the movable rod when the pipe is installed, and the installation is more stable.

[0031] In summary, the present invention has the following beneficial effects:

[0032] 1. The scheme of the present invention uses HDPE resin as raw material, adds nano copper catalyst and polybutylene adipate / terephthalate PBAT, polylactic acid PLA, polyhydroxyalkanoate PHA biodegradable materials, activates the nano copper catalyst by 60-90°C high temperature water and then cooperates with the above-mentioned degradation materials to degrade the sewage pipe dirt, which can quickly control the degradation of the inner layer of the pipe, ensure that the pipe dirt is cleanly treated, and at the same time ensure that the plastic pipe system meets the relevant standards and operates normally;

[0033] 2. During the degradation process, just pass hot water into the silt-filled pipe and soak it for a period of time to complete the pipe cleaning, which saves time and effort and has significant after-sales economic benefits;

[0034] 3. With the special pipeline design structure, the water supply and drainage pipelines are more resistant to high temperatures during use, and can be more firmly installed in the designed pipeline installation line. With the customized pipeline preparation method and process, the service life of the pipeline can be extended and the replacement cost of the water supply and drainage pipeline can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] FIG1 is a cross-sectional view of a HDPE water supply and drainage pipeline for dredging of the present invention;

[0036] FIG2 is an enlarged structural schematic diagram of point A in FIG1 ;

[0037] Figure 3 is a schematic diagram of the fixed plate structure;

[0038] Among them, 1. functional inner layer; 2. heat-resistant outer layer; 3. protective cotton; 4. pipe shell; 5. fixed plate; 6. movable rod; 7. limiting spring; 8. stabilizing spring; 9. protective pad. DETAILED DESCRIPTION

[0039] The following specific embodiments are merely explanations of the present invention and are not limitations of the present invention. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, such modifications are protected by the patent law as long as they are within the scope of the claims of the present invention.

[0040] Example 1

[0041] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 30 parts of HDPE high-density polyethylene resin, 5 parts of linear low-density polyethylene, 5 parts of polybutylene adipate / terephthalate PBAT, 5 parts of polylactic acid PLA, 5 parts of polyhydroxyalkanoate PHA, 0.5 parts of nano copper, lubricants including fluorine-containing polymer PPA, calcium stearate and zinc stearate, wherein the fluorine-containing polymer PPA is 0.5 parts, calcium stearate is 1 part, zinc stearate is 1 part, vinyl trimethoxy silane is 0.05 parts, and nano silicon dioxide nSiO25 parts are mixed and melt-granulated for standby use.

[0042] Step S2 is the preparation of the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: a total of 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene are prepared, of which 1 part is reduced graphene oxide and the rest is PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of the reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by the Hummers method, and the prepared graphene oxide is pickled with 3% H2SO4 solution and 0.5% H2O2 solution for 20 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 10 times; the pickled graphene oxide is dried at 90°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 80 seconds to obtain reduced graphene oxide rGO.

[0043] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 140°C; the extrusion temperature of the heat-resistant outer layer is 165°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:6.

[0044] The water supply and drainage pipe structure of this embodiment only includes a two-layer structure of a temperature-resistant outer layer 2 and an active inner layer 1 .

[0045] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 60℃, the immersion time was 48h, and the sewage was discharged after the immersion was completed.

[0046] Example 2

[0047] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 60 parts of HDPE high-density polyethylene resin, 20 parts of linear low-density polyethylene, 10 parts of polybutylene adipate / terephthalate PBAT, 10 parts of polylactic acid PLA, 10 parts of polyhydroxyalkanoate PHA, 10 parts of nano copper, lubricants including fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 2 parts, calcium stearate is 8 parts, zinc stearate is 8 parts, vinyl trimethoxy silane is 0.1 parts, and nano silicon dioxide nSiO2 10 parts are mixed and melt-granulated for standby use.

[0048] Step S2 is the preparation of the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: a total of 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene are prepared, of which 5 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of the reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by the Hummers method, and the prepared graphene oxide is pickled with 3% H2SO4 solution and 0.5% H2O2 solution for 28 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 15 times; the pickled graphene oxide is dried at 105°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 150 seconds to obtain reduced graphene oxide rGO.

[0049] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 160°C; the extrusion temperature of the heat-resistant outer layer is 185°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:19.

[0050] The water supply and drainage pipe structure of this embodiment only includes a two-layer structure of a temperature-resistant outer layer 2 and an active inner layer 1 .

[0051] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 90℃, the immersion time was 1h, and the sewage was discharged after the immersion was completed.

[0052] Example 3

[0053] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 40 parts of HDPE high-density polyethylene resin, 10 parts of linear low-density polyethylene, 6 parts of polybutylene adipate / terephthalate PBAT, 6 parts of polylactic acid PLA, 6 parts of polyhydroxyalkanoate PHA, 3 parts of nano copper, lubricants including fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 1.2 parts, calcium stearate is 5 parts, zinc stearate is 5 parts, vinyl trimethoxy silane is 0.07 parts, and nano silicon dioxide nSiO2 4.6 parts are mixed and melt-granulated for standby use.

[0054] Step S2 is the preparation of the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: a total of 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene are prepared, of which 3.3 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of the reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by the Hummers method, and the prepared graphene oxide is pickled with 3% H2SO4 solution and 0.5% H2O2 solution for 24 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 14 times; the pickled graphene oxide is dried at 98°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 130 seconds to obtain reduced graphene oxide rGO.

[0055] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 155°C; the extrusion temperature of the heat-resistant outer layer is 175°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:12.

[0056] Furthermore, as shown in Figures 1 to 3, the structure of the water supply and drainage pipe of this embodiment is shown. The outer side of the heat-resistant outer layer 2 is fixedly covered with protective cotton 3, which is made of high-temperature resistant material. The outer side of the protective cotton 3 is fixedly installed with a pipe shell 4, and the outer side of the heat-resistant outer layer 2 is also fixedly installed with a movable rod 6, and the top of the movable rod 6 is fixedly installed with a fixed plate 5, and the movable rod 6 is made of a telescopic structure; the active inner layer 1 and the heat-resistant outer layer 2 are arranged in the innermost circle of the pipe, and the outer side of the heat-resistant outer layer 2 is fixedly installed with a limiting spring 7, and the top of the limiting spring 7 is fixedly connected to the inner side of the pipe shell 4, and the pipe shell 4 is made of elastic material; the limiting spring 7 is sleeved on the outer side of the movable rod 6; the top of the fixed plate 5 is fixedly installed with a stabilizing spring leaf 8, and the top of the stabilizing spring leaf 8 is fixedly installed with an elastic protective pad 9.

[0057] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 75℃, the immersion time was 36h, and the sewage was discharged after the immersion was completed.

[0058] Example 4

[0059] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 50 parts of HDPE high-density polyethylene resin, 15 parts of linear low-density polyethylene, 7 parts of polybutylene adipate / terephthalate PBAT, 7 parts of polylactic acid PLA, 5 parts of polyhydroxyalkanoate PHA, 3.9 parts of nano copper, lubricants including fluorine-containing polymer PPA, calcium stearate and zinc stearate, wherein the fluorine-containing polymer PPA is 0.8 parts, calcium stearate is 4 parts, zinc stearate is 4 parts, vinyl trimethoxy silane is 0.09 parts, and nano silicon dioxide nSiO2 8 parts are mixed and melt-granulated for standby use.

[0060] Step S2 is the preparation of the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: a total of 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene are prepared, of which 2 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of the reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by the Hummers method, and the prepared graphene oxide is pickled with 3% H2SO4 solution and 0.5% H2O2 solution for 25 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 11 times; the pickled graphene oxide is dried at 95°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 120 seconds to obtain reduced graphene oxide rGO.

[0061] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 150°C; the extrusion temperature of the heat-resistant outer layer is 180°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:8.

[0062] The water supply and drainage pipe structure of this embodiment only includes a two-layer structure of a temperature-resistant outer layer 2 and an active inner layer 1 .

[0063] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 65℃, the immersion time was 24h, and the sewage was discharged after the immersion was completed.

[0064] Example 5

[0065] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 50 parts of HDPE high-density polyethylene resin, 15 parts of linear low-density polyethylene, 7 parts of polybutylene adipate / terephthalate PBAT, 7 parts of polylactic acid PLA, 5 parts of polyhydroxyalkanoate PHA, 3.9 parts of nano copper, lubricants including fluorine-containing polymer PPA, calcium stearate and zinc stearate, wherein the fluorine-containing polymer PPA is 0.8 parts, calcium stearate is 4 parts, zinc stearate is 4 parts, vinyl trimethoxy silane is 0.09 parts, and nano silicon dioxide nSiO2 8 parts are mixed and melt-granulated for standby use.

[0066] Step S2 is the preparation of the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: a total of 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene are prepared, of which 2 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of the reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by the Hummers method, and the prepared graphene oxide is pickled with 3% H2SO4 solution and 0.5% H2O2 solution for 25 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 11 times; the pickled graphene oxide is dried at 95°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 120 seconds to obtain reduced graphene oxide rGO.

[0067] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 150°C; the extrusion temperature of the heat-resistant outer layer is 170°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:15.

[0068] The water supply and drainage pipe structure of this embodiment only includes a two-layer structure of a temperature-resistant outer layer 2 and an active inner layer 1 .

[0069] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 80℃, the immersion time was 12h, and the sewage was discharged after the immersion was completed.

[0070] Example 6

[0071] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 48 parts of HDPE high-density polyethylene resin, 14 parts of linear low-density polyethylene, 8 parts of polybutylene adipate / terephthalate PBAT, 6 parts of polylactic acid PLA, 7 parts of polyhydroxyalkanoate PHA, 6 parts of nano copper, lubricants including fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 1.2 parts, calcium stearate is 4.2 parts, zinc stearate is 4.2 parts, vinyl trimethoxy silane is 0.065 parts, and nano silicon dioxide nSiO2 is 6.6 parts. Mix and melt granulate for later use.

[0072] Step S2 is the preparation of the heat-resistant outer layer raw materials for the drainage pipe: prepare 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene, of which 3.7 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by Hummers method, and the prepared graphene oxide is acid-washed with 3% H2SO4 solution and 0.5% H2O2 solution for 24 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 12 times; the acid-washed graphene oxide is dried at 100°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 120 seconds to obtain reduced graphene oxide rGO.

[0073] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 155°C; the extrusion temperature of the heat-resistant outer layer is 180°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:9.

[0074] Furthermore, as shown in Figures 1 to 3, the structure of the water supply and drainage pipe of this embodiment is shown. The outer side of the heat-resistant outer layer 2 is fixedly covered with protective cotton 3, which is made of high-temperature resistant material. The outer side of the protective cotton 3 is fixedly installed with a pipe shell 4, and the outer side of the heat-resistant outer layer 2 is also fixedly installed with a movable rod 6, and the top of the movable rod 6 is fixedly installed with a fixed plate 5, and the movable rod 6 is made of a telescopic structure; the active inner layer 1 and the heat-resistant outer layer 2 are arranged in the innermost circle of the pipe, and the outer side of the heat-resistant outer layer 2 is fixedly installed with a limiting spring 7, and the top of the limiting spring 7 is fixedly connected to the inner side of the pipe shell 4, and the pipe shell 4 is made of elastic material; the limiting spring 7 is sleeved on the outer side of the movable rod 6; the top of the fixed plate 5 is fixedly installed with a stabilizing spring leaf 8, and the top of the stabilizing spring leaf 8 is fixedly installed with an elastic protective pad 9.

[0075] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 80℃, the immersion time was 6h, and the sewage was discharged after the immersion was completed.

[0076] Example 7

[0077] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 48 parts of HDPE high-density polyethylene resin, 14 parts of linear low-density polyethylene, 8 parts of polybutylene adipate / terephthalate PBAT, 6 parts of polylactic acid PLA, 7 parts of polyhydroxyalkanoate PHA, 6 parts of nano copper, lubricants including fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 1.2 parts, calcium stearate is 4.2 parts, zinc stearate is 4.2 parts, vinyl trimethoxy silane is 0.065 parts, and nano silicon dioxide nSiO2 is 6.6 parts. Mix and melt granulate for later use.

[0078] Step S2 is the preparation of the heat-resistant outer layer raw materials for the drainage pipe: prepare 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene, of which 3.7 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by Hummers method, and the prepared graphene oxide is acid-washed with 3% H2SO4 solution and 0.5% H2O2 solution for 24 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 12 times; the acid-washed graphene oxide is dried at 100°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 120 seconds to obtain reduced graphene oxide rGO.

[0079] Step S3 co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 155°C; the extrusion temperature of the heat-resistant outer layer is 180°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:9.

[0080] Furthermore, as shown in Figures 1 to 3, the structure of the water supply and drainage pipe of this embodiment is shown. The outer side of the heat-resistant outer layer 2 is fixedly covered with protective cotton 3, which is made of high-temperature resistant material. The outer side of the protective cotton 3 is fixedly installed with a pipe shell 4, and the outer side of the heat-resistant outer layer 2 is also fixedly installed with a movable rod 6, and the top of the movable rod 6 is fixedly installed with a fixed plate 5, and the movable rod 6 is made of a telescopic structure; the active inner layer 1 and the heat-resistant outer layer 2 are arranged in the innermost circle of the pipe, and the outer side of the heat-resistant outer layer 2 is fixedly installed with a limiting spring 7, and the top of the limiting spring 7 is fixedly connected to the inner side of the pipe shell 4, and the pipe shell 4 is made of elastic material; the limiting spring 7 is sleeved on the outer side of the movable rod 6; the top of the fixed plate 5 is fixedly installed with a stabilizing spring leaf 8, and the top of the stabilizing spring leaf 8 is fixedly installed with an elastic protective pad 9.

[0081] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 80℃, the immersion time was 24h, and the sewage was discharged after the immersion was completed.

[0082] Comparative Example 1

[0083] Different from the embodiment, no nano copper catalyst was added in this comparative example;

[0084] Step S1 prepares the raw materials for the inner layer of the water supply and drainage pipe: 48 parts of HDPE high-density polyethylene resin, 14 parts of linear low-density polyethylene, 8 parts of polybutylene adipate / terephthalate PBAT, 6 parts of polylactic acid PLA, 7 parts of polyhydroxyalkanoate PHA, and lubricants including fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 1.2 parts, calcium stearate is 4.2 parts, zinc stearate is 4.2 parts, vinyl trimethoxy silane is 0.065 parts, and nano silicon dioxide nSiO2 is 6.6 parts. Mix and melt granulate for later use.

[0085] Step S2 is the preparation of the heat-resistant outer layer raw materials for the drainage pipe: prepare 100 parts of reduced graphene oxide and PE-RT high temperature resistant polyethylene, of which 3.7 parts are reduced graphene oxide and the rest are PE-RT high temperature resistant polyethylene. After mixing, they are melt-granulated for standby use. The preparation process of reduced graphene oxide is to first preliminarily prepare graphene oxide with graphite oxide attached by Hummers method, and the prepared graphene oxide is acid-washed with 3% H2SO4 solution and 0.5% H2O2 solution for 24 hours, and then washed with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washings is 12 times; the acid-washed graphene oxide is dried at 100°C to a constant weight, then resuspended and ultrasonicated for 24 hours to obtain graphene oxide with a completely reduced stratum corneum, and finally the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 120 seconds to obtain reduced graphene oxide rGO.

[0086] Step S3 co-extrusion molding: the prepared inner and outer layer mixed raw materials are co-extruded to form a double-layer structure in the tube, wherein the active inner layer plastic pellets and the heat-resistant outer layer plastic pellets are molded by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the active inner layer is 155°C; the extrusion temperature of the heat-resistant outer layer is 180°C; after co-extrusion, the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer are in the ratio of 1:9.5.

[0087] The water supply and drainage pipe structure only includes an inner functional layer 1 and a temperature-resistant outer layer 2.

[0088] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 80℃, the immersion time was 36h, and the sewage was discharged after the immersion was completed.

[0089] Comparative Example 2

[0090] The same raw material formula and pipeline structure as those in comparative example 1 are used, except that in the desilting effect test of water supply and drainage pipes, high-temperature water above 95° C. is introduced during the test, and the immersion time is 24 hours.

[0091] Comparative Example 3

[0092] Different from the above embodiment, in step S1 of this comparative example, 46 parts of HDPE high-density polyethylene resin, 12 parts of linear low-density polyethylene resin, 17 parts of lubricant, 8 parts of one of polybutylene adipate / terephthalate PBAT, polylactic acid PLA, and polyhydroxyalkanoate PHA are used as biodegradable materials, and 5 parts of nano copper catalyst are used to prepare the inner layer, and the subsequent heat-resistant outer layer and co-extrusion steps are the same as those in Example 6.

[0093] Before the desilting effect test of water supply and drainage pipes, the inner wall of the pipes was artificially coated with dirt that was difficult to clean, and a 1m sample was taken for the test. The temperature of the water introduced during the test was 80℃, the immersion time was 24h, and the sewage was discharged after the immersion was completed.

[0094] For the water supply and drainage pipes prepared in the above embodiments and comparative examples, firstly, according to the implementation standard GB / T13663.2-2018, HDPE, dn160SDR11*14.6mm, 1.6MPa pipes were used for verification, and the degradation and cleaning of dirt in the pipeline were observed every 3 hours; the static hydraulic strength tests of 20℃ / 100h / 12.0MPa, 80℃ / 165h / 5.4MPa and 80℃ / 1000h / 5.0MPa were performed on the pipe samples of the embodiment according to the national standard.

[0095] The dirt removal observation results are shown in Table 1 below, where a means that the dirt is completely removed, b means that most of the dirt is removed, c means that the dirt is partially removed, and d means that the dirt cleaning effect is basically not achieved.

[0096] Table 1 Observation results of the dirt removal process

[0097]

[0098] The following conclusions can be drawn from Table 1:

[0099] It can be seen from the examples 1 to 7 that the degradation speed and time of the dirt in the HDPE plastic pipe for desilting and drainage can be controlled with the different raw material ratios and the ratio of the thickness of the two-layer pipe wall in step S1. In example 6, the dirt has been basically completely degraded after the pipe has been immersed for 3 hours, with high efficiency and high speed. To control the degradation speed of the pipe dirt faster, corresponding adjustments and modifications can be made according to the test conditions in example 6. In example 7, the dirt has been completely degraded after the third hour, but the immersion is still in progress. After observing the pipe samples after the test, it is found that the inner layer of dirt has been completely degraded and fallen off, while the heat-resistant outer layer has not decomposed. It can be concluded that this scheme is safe and feasible. Since example 1 was immersed for only 1 hour, the decomposition time of the dirt was insufficient and the purification was incomplete. According to the degradation speed, the remaining examples are ranked as example 6> example 2> example 4> example 5. According to this result, the pipe material preparation and the inner wall thickness can be reasonably adjusted and applied to actual scenarios. In addition, the example using a special pipe structure is more stable during installation and has better heat resistance.

[0100] In Comparative Example 1, no nano-copper catalyst was added to the pipe formula, and its dirt removal rate became poor. Although biodegradable materials were added, only partial dirt removal could be achieved after immersion for 24 hours. It can be concluded that the use of nano-copper catalyst is a crucial step. Subsequently, Comparative Example 1 was also carried out under low-temperature water conditions, and its degradation effect was even worse; in Comparative Example 2, although the water temperature was increased, the final result of dirt degradation was not optimized; in Comparative Example 3, only one biodegradable material was used in combination with the nano-copper catalyst, and its final degradation result was slightly better than the previous two comparative examples, but far inferior to other embodiments.

[0101] In addition, the pipe samples of Examples 1-7 were subjected to hydrostatic strength tests at 20°C / 100h / 12.0MPa, 80°C / 165h / 5.4MPa and 80°C / 1000h / 5.0MPa according to national standards, and the results were all qualified.

Claims

1. A HDPE water supply and drainage plastic pipe system for dredging, characterized in that: The HDPE water supply and drainage plastic pipe for dredging comprises an active inner layer and a heat-resistant outer layer, wherein the heat-resistant outer layer is a performance supporting layer, the active inner layer is a main degradation active layer, and the heat-resistant outer layer serves as a performance supporting protective layer for the active inner layer; the active inner layer comprises HDPE and biodegradable materials, lubricants and nano copper catalysts, and the thickness of the active inner layer and the wall thickness of the heat-resistant outer layer have a ratio ranging from (1:6) to (1:19).

2. The HDPE water supply and drainage plastic pipe system for dredging according to claim 1 is characterized by: The raw materials of the inner layer include 30-60 parts of HDPE high-density polyethylene resin, 5-20 parts of linear low-density polyethylene, 5-10 parts of polybutylene adipate / terephthalate PBAT, 5-10 parts of polylactic acid PLA, 5-10 parts of polyhydroxyalkanoate PHA, and 0.5-10 parts of nano copper. The lubricant includes fluorinated polymer PPA, calcium stearate and zinc stearate, wherein the fluorinated polymer PPA is 0.5-2 parts, calcium stearate is 1-8 parts, and zinc stearate is 1-8 parts, and all parts are by mass, wherein the mass is not limited to 100 parts.

3. A HDPE water supply and drainage plastic pipe system for dredging according to claim 2, characterized in that: Furthermore, the HDPE high-density polyethylene resin is 48 parts, the linear low-density polyethylene is 14 parts, the polybutylene adipate / terephthalate PBAT is 8 parts, the polylactic acid PLA is 6 parts, the polyhydroxyalkanoate PHA is 7 parts, the nano copper is 6 parts, and the lubricant includes fluoropolymer PPA, calcium stearate and zinc stearate, wherein the fluoropolymer PPA is 1.2 parts, the calcium stearate is 4.2 parts, and the zinc stearate is 4.2 parts.

4. The HDPE water supply and drainage plastic pipe system for dredging according to claim 1 is characterized by: The production of HDPE water supply and drainage plastic pipes for dredging includes the following process steps: Step S1: preparing the raw materials for the inner layer of the water supply and drainage pipe: premixing HDPE high-density polyethylene resin, linear low-density polyethylene resin, polybutylene adipate / terephthalate PBAT, polylactic acid PLA, polyhydroxyalkanoate PHA, lubricant and nano copper in a suitable proportion and then melt-granulating them for later use; Step S2: preparing the raw materials for the heat-resistant outer layer of the water supply and drainage pipe: preparing reduced graphene oxide and PE-RT high-temperature resistant polyethylene, mixing them in proportion, and then melting and granulating them for later use; Step S3: co-extrusion molding: the inner and outer layer mixed raw materials obtained in step S1 and step S2 are co-extruded to form a double-layer structure inside the tube.

5. The HDPE plastic pipe system for water supply and drainage for dredging according to claim 4 is characterized by: Furthermore, the raw materials of step S1 also include vinyltrimethoxysilane and nano-silicon dioxide nSiO2, and the vinyltrimethoxysilane is used as a carrier to load the nano-silicon dioxide nSiO2; the mass fractions of vinyltrimethoxysilane and nano-silicon dioxide are 0.05-0.1 parts and 5-10 parts respectively.

6. The HDPE plastic pipe system for water supply and drainage for dredging according to claim 4, characterized in that: The preparation process of reduced graphene oxide in step S2 is to first preliminarily prepare graphene oxide with graphite oxide attached by Hummers method, pickle the prepared graphene oxide with 3% H2SO4 solution and 0.5% H2O2 solution for 20-28h, and then wash it with the same acid solution for multiple times to make part of the graphite oxide fall off, and the number of washing times is 10-15 times; the pickled graphene oxide is dried at 90-105°C to a constant weight, and then resuspended and ultrasonicated for 24h to obtain graphene oxide with a completely reduced stratum corneum; finally, the graphene oxide GO obtained by the above process is thermally reduced at 1000°C for 80-150 seconds to obtain reduced graphene oxide rGO.

7. The HDPE water supply and drainage plastic pipe system for dredging according to claim 4 is characterized by: The total mass fraction of reduced graphene oxide and PE-RT high temperature resistant polyethylene in step S2 is 100 parts; wherein the mass fraction of reduced graphene oxide is 1-5 parts, and the rest is PE-RT high temperature resistant polyethylene.

8. The HDPE water supply and drainage plastic pipe system for dredging according to claim 4, characterized in that: In step S3, the functional inner layer plastic pellets and the heat-resistant outer layer plastic pellets obtained in step S1 and step S2 are formed by a co-extrusion extruder. During the extrusion process, the extrusion temperature of the functional inner layer is 140-160° C.; the extrusion temperature of the heat-resistant outer layer is 165-185° C.

9. The HDPE water supply and drainage plastic pipe system for dredging according to claim 1, characterized in that: In addition to the functional inner layer and the temperature-resistant outer layer, the water supply and drainage plastic pipe also includes the following structures: The outer side of the heat-resistant outer layer is fixedly covered with protective cotton, which is made of high-temperature resistant material. The outer side of the protective cotton is fixedly installed with a pipeline shell. The outer side of the heat-resistant outer layer is also fixedly installed with a movable rod, and the top of the movable rod is fixedly installed with a fixed plate. The movable rod is made of a telescopic structure. The functional inner layer and the heat-resistant outer layer are arranged at the innermost circle of the pipeline, a limiting spring is fixedly installed on the outer side of the heat-resistant outer layer, the top end of the limiting spring is fixedly connected to the inner side of the pipeline shell, and the pipeline shell is made of elastic material; the limiting spring is sleeved on the outer side of the movable rod; A stabilizing spring is fixedly installed on the top of the fixing plate, and an elastic protective pad is fixedly installed on the top of the stabilizing spring.

10. A HDPE water supply and drainage plastic pipe system for dredging, characterized in that: According to the HDPE water supply and drainage plastic pipe system for dredging according to any one of claims 1 to 9, it can be applied to the preparation and cleaning of plastic pipes such as water supply and drainage by combining the pipe structure and adjusting the flushing temperature, the inner pipe formula and the thickness ratio of the two layers. During the pipe dredging process, high-temperature water is introduced into the water supply and drainage pipe for immersion, the water temperature is controlled at 60-90°C, and the immersion time is 1-48h. The nano copper catalyst is activated by high temperature to decompose the inner layer material, and the degraded internal dirt and the inner layer material can be dissolved in the sewage and stripped off by water, and flushed out of the pipe with the water flow to complete the dredging process.